[0031] A method for recycling titanium-containing fine material, comprising the steps of:
[0032] S1, titanium-containing fine material molding
[0033] Feed the fine-grade titanium slag, water, and starch into the mixer according to the weight ratio of 1:0.01:0.01 for mixing, and then send it to the vacuum extrusion equipment for extrusion molding to obtain the molding material;
[0034] S2, calcination of molding materials
[0035] The formed material is placed in a rotary kiln, and the by-product gas of the titanium slag furnace is used to burn and heat for calcination. The calcination temperature is 800 ° C, and the calcination time is 1 h to obtain the calcined material;
[0036] S3, broken classification
[0037] S3.1, sending the calcined material into the roller mill for crushing to obtain the crushed material;
[0038] S3.2, send the crushed material to the screening device, and screen to obtain three groups of large particle material, qualified particle material,...
Embodiment 2
[0040] A method for recycling titanium-containing fine material, comprising the steps of:
[0041] S1, titanium-containing fine material molding
[0042] Feed the fine-grade natural rutile, water, and PVA into the mixer according to the weight ratio of 1:0.05:0.1 for mixing, and then send them into the non-vacuum extrusion equipment for extrusion molding to obtain the molding materials;
[0043] S2, calcination of molding materials
[0044] The formed material is placed in a rotary kiln, and the by-product gas of the titanium slag furnace is used to burn and heat for calcination. The calcination temperature is 1000 ° C, and the calcination time is 5 h to obtain the calcined material;
[0045] S3, broken classification
[0046] S3.1, sending the calcined material into the roller mill for crushing to obtain the crushed material;
[0047] S3.2, send the crushed material to the screening device, and screen to obtain three groups of large particle material, qualified particle ma...
Embodiment 3
[0049] A method for recycling titanium-containing fine material, comprising the steps of:
[0050] S1, titanium-containing fine material molding
[0051] Send the fine grade artificial rutile, water, and sodium humate into the mixer according to the weight ratio of 1:0.1:0.05 for mixing, and then send them into the non-vacuum extrusion equipment for extrusion molding to obtain the molding material;
[0052] S2, calcination of molding materials
[0053] The formed material is placed in a rotary kiln, and the by-product gas of the titanium slag furnace is used to burn and heat for calcination. The calcination temperature is 1100 ° C, and the calcination time is 3 h to obtain the calcined material;
[0054] S3, broken classification
[0055] S3.1, sending the calcined material into the roller mill for crushing to obtain the crushed material;
[0056] S3.2, send the crushed material to the screening device, and screen to obtain three groups of large particle material, qualified...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com