Method for preparing zinc oxide for sealing ring
A zinc oxide and sealing ring technology, applied in the direction of zinc oxide/zinc hydroxide, etc., can solve the problems of uneven texture, poor dispersion, and poor weather resistance of sealing rings, and achieve strong wear resistance, good lubricity, and improved Effect of Vulcanization Rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] A method for preparing zinc oxide for sealing ring, comprising the following steps:
[0021] Step 1, weigh the following components by weight: 50 parts of ordinary zinc oxide, 10 parts of nano titanium dioxide, 1 part of chitosan, 2 parts of phthalate coupling agent, 5 parts of nano white carbon black, 5 parts of polyethylene 1 part of plasticizer;
[0022] Step 2, mixing polyethylene and a plasticizer, and plasticizing for 10 minutes to obtain mixture A;
[0023] Step 3, mixing ordinary zinc oxide, chitosan, nano-titanium dioxide, and nano-white carbon black into a muffle furnace for sintering for 1-2 hours, and then transferring to a ball mill to grind the mixture B;
[0024] Step 4, mix mixture B, mixture A, and phthalate coupling agent, put into a ball mill and stir at a speed of 120 rpm to obtain material A;
[0025] Step 5, transfer material A to a calciner for calcination to obtain the required zinc oxide.
[0026] Wherein, the temperature of the plasticizing ...
Embodiment 2
[0031] A method for preparing zinc oxide for sealing ring, comprising the following steps:
[0032] Step 1, weigh the following components by weight: 68 parts of ordinary zinc oxide, 15 parts of nano titanium dioxide, 3 parts of chitosan, 4 parts of phthalate coupling agent, 6 parts of nano white carbon black, 12 parts of polyethylene , 2 parts of plasticizer;
[0033] Step 2, mixing polyethylene and a plasticizer, and plasticizing for 12 minutes to obtain mixture A;
[0034] Step 3, mixing ordinary zinc oxide, chitosan, nano-titanium dioxide, and nano-white carbon black into a muffle furnace for sintering for 2 hours, then transferring to a ball mill to grind the mixture B;
[0035] Step 4, mix mixture B, mixture A, and phthalate coupling agent, put into a ball mill and stir at a speed of 150 rpm to obtain material A;
[0036] Step 5, transfer material A to a calciner for calcination to obtain the desired zinc oxide.
[0037] Wherein, the temperature of the plasticizing tr...
Embodiment 3
[0042] A method for preparing zinc oxide for sealing ring, comprising the following steps:
[0043] Step 1, take the following components by weight: 75 parts of ordinary zinc oxide, 18 parts of nano titanium dioxide, 4 parts of chitosan, 5 parts of phthalate coupling agent, 8 parts of nano white carbon black, 15 parts of polyethylene , 3 parts of plasticizer;
[0044] Step 2, mixing polyethylene and a plasticizer, and plasticizing for 10-15 minutes to obtain mixture A;
[0045] Step 3, mixing ordinary zinc oxide, chitosan, nano-titanium dioxide, and nano-white carbon black into a muffle furnace for sintering for 1-2 hours, and then transferring to a ball mill to grind the mixture B;
[0046] Step 4, mix mixture B, mixture A, and phthalate coupling agent, put into a ball mill and stir at a speed of 180 rpm to obtain material A;
[0047] Step 5, transfer material A to a calciner for calcination to obtain the desired zinc oxide.
[0048] Wherein, the temperature of the plastic...
PUM
Property | Measurement | Unit |
---|---|---|
elongation at break | aaaaa | aaaaa |
elongation at break | aaaaa | aaaaa |
elongation at break | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com