A technology of attapulgite and attapulgite powder, applied in fertilizer mixture, application, organic fertilizer and other directions, can solve the problems of weak non-metallic mineral processing industry foundation, low level of development and utilization, waste of resources, etc., to improve the quality of agricultural products and achieve good results , the effect of increasing production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0056] An improved synergistic method for mixing attapulgite, comprising the following preparation steps:
[0057] A. Raw ore crushing
[0058] Crushing the attapulgite ore, the crushing mesh is 30 mesh-60 mesh;
[0059] B. Acidification treatment
[0060] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0061] C. Drying and sieving
[0062] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0063] D. Baking
[0064] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time is 45-120 ...
Embodiment 2
[0072] An improved synergistic method for mixing attapulgite, comprising the following preparation steps:
[0073] A. Raw ore crushing
[0074] Crushing the attapulgite ore, the crushing mesh is 30 mesh-60 mesh;
[0075] B. Acidification treatment
[0076] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0077] C. Drying and sieving
[0078] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0079] D. Baking
[0080] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time is 45-12...
Embodiment 3
[0088] An improved synergistic method for mixing attapulgite, comprising the following preparation steps:
[0089] A. Raw ore crushing
[0090] Crushing the attapulgite ore, the crushing mesh is 30 mesh-60 mesh;
[0091] B. Acidification treatment
[0092] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0093] C. Drying and sieving
[0094] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0095] D. Baking
[0096] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time is 45-12...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com