Jelly-paraffin-containing phase transition energy storage perlite and self-temperature-adjustment phase transition mortar
A phase change energy storage and perlite technology, which is applied in the field of building materials, can solve the problems of phase change materials and phase change mortar leakage preparation process, complexity and other problems, and achieve good construction stability, less leakage and good phase change stability. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] 1. Preparation of phase change perlite:
[0021] 1. Take 150 grams of paraffin wax at 25°C, add 3 grams of thermoplastic styrene-butadiene rubber and styrene-butadiene thermoplastic elastomer to the paraffin wax, mix evenly, raise the temperature to 90-100°C, stir evenly, and make jelly for 10 minutes.
[0022] 2. Take 100 grams of 2-3mm expanded turpentine rock, put it in a three-necked flask, control the water bath at 90°C, turn on the vacuum, and stir at a low speed. When the temperature of the material in the kettle rises to more than 80° C., inhale the liquid jelly wax obtained in step 1, slowly inhale, start timing after all inhalation, and continue vacuum stirring for 100 min.
[0023] 3. Add 5 grams of sodium dodecylsulfonate to the material obtained in step 2, stir and react in vacuum for 60 minutes, then raise the temperature to 100° C., and react in vacuum for 1 hour.
[0024] 4. Add 30 grams of acidic silica sol to the material obtained in step 3, and stir ...
Embodiment 2
[0030] 1. Preparation of phase change perlite:
[0031] 1. Take 200 grams of paraffin wax at 20°C, add 2.7 grams of thermoplastic styrene-butadiene rubber and styrene-butadiene thermoplastic elastomer to the paraffin wax, mix evenly, raise the temperature to 90-100°C, stir evenly, and make jelly for 10 minutes.
[0032]2. Take 100 grams of 2-3mm expanded turpentine rock, put it in a three-necked flask, control the water bath at 90°C, turn on the vacuum, and stir at a low speed. When the temperature of the material in the kettle rises to more than 80° C., inhale the liquid jelly wax obtained in step 1, slowly inhale, start timing after all inhalation, and continue vacuum stirring for 100 min.
[0033] 3. Add 5 grams of sodium dodecylsulfonate to the material obtained in step 2, stir and react in vacuum for 60 minutes, then raise the temperature to 100° C., and react in vacuum for 1 hour.
[0034] 4. Add 30 grams of acidic silica sol to the material obtained in step 3, and stir...
Embodiment 3
[0040] 1. Preparation of phase change perlite:
[0041] 1. Take 150 grams of paraffin wax at 30°C, add 3.5 grams of thermoplastic styrene-butadiene rubber and styrene-butadiene thermoplastic elastomer to the paraffin wax, mix evenly, raise the temperature to 100-120°C, stir evenly, and make jelly for 10 minutes.
[0042] 2. Take 100 grams of 2-3mm expanded turpentine rock, put it in a three-necked flask, control it at 110°C, turn on the vacuum, and stir at a low speed. When the temperature of the material in the kettle rises to greater than 100° C., inhale the liquid jelly wax obtained in step 1, slowly inhale, start timing after all inhalation, and continue vacuum stirring for 100 min.
[0043] 3. Add 5 grams of sodium dodecylsulfonate to the material obtained in step 2, stir and react in vacuum for 60 minutes, then raise the temperature to 100° C., and react in vacuum for 1 hour.
[0044] 4. Add 30 grams of acidic silica sol to the material obtained in step 3, and stir at a...
PUM
Property | Measurement | Unit |
---|---|---|
phase transition temperature | aaaaa | aaaaa |
latent heat | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com