Preparation method for solvent-free root-puncture-resistant waterproof polyurethane paint
A polyurethane waterproof and solvent-free technology, applied in the field of polyurethane coatings, can solve problems such as plant death, poor root thorn resistance, and environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] Component A consists of the following components by weight:
[0043] Raw material name Weight ratio
[0044] Polyether diol 300 parts
[0045] Polyether triol 80 parts
[0046] Toluene diisocyanate (TDI) 119 parts
[0047] Stabilizer 1 part
[0048] Component B consists of the following components by weight:
[0049] Raw material name Weight ratio
[0050] Polyether triol 500 parts
[0051] Dioctyl phthalate 250 parts
[0053] Ground calcium carbonate 100 parts
[0054] Cross-linking agent 19 parts
[0055] Catalyst 0.4 parts
[0056] Thixotropic agent 6 parts
[0057] Red iron oxide 4 parts
[0058] Chemical root inhibitor 0.6 parts
[0059] Other 10 copies
[0060] Process engineering:
[0061] (1) Add 300 parts of polyether diol, 80 parts of polyether triol and 1 part of stabilizer into the reaction kettle.
[0062] (2) Raise the temperature to 80°C to 100°C and start stirring.
[0063] (3) Vacuum dehydration and degass...
Embodiment 2
[0073] Component A consists of the following components by weight:
[0074] Raw material name Weight ratio
[0075] Polyether diol 250 parts
[0076] Polyether triol 100 parts
[0077] Toluene diisocyanate (TDI) 147 parts
[0078] Stabilizer 3 parts
[0079] Component B consists of the following components by weight:
[0080] Raw material name Weight ratio
[0081] Polyether triol 550 parts
[0082] Dioctyl phthalate 200 parts
[0084] Ground Calcium Carbonate 110 parts
[0085] Cross-linking agent 19 parts
[0086] Catalyst 0.4 parts
[0087] Thixotropic agent 4 parts
[0088] Iron oxide red 6 parts
[0089] Chemical root inhibitor 0.6 parts
[0090] Other 10 copies
[0091] Process engineering:
[0092] (1) Add 250 parts of polyether diol, 100 parts of polyether triol and 3 parts of stabilizer into the reaction kettle.
[0093] (2) Raise the temperature to 80°C to 100°C and start stirring.
[0094] (3) Vacuum dehydration and dega...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com