A low-temperature cement early strength agent for well cementing and cement containing it
An early-strength agent and low-temperature technology, applied in the direction of drilling compositions, chemical instruments and methods, etc., can solve problems such as the decline in the ability to resist sulfate corrosion, the inability to meet the needs of early-strength agents, and the increase in cement stone volume shrinkage, etc. Achieve superior low temperature early strength and compressive strength, excellent acid and alkali corrosion resistance, and reduce viscosity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] Weigh each component according to the following ratio: 25 parts of sodium sulfate, 6 parts of sodium nitrate, 4 parts of ferrous sulfate, 0.2 part of diethanolamine, 0.5 part of triethanolamine, 1.2 parts of water reducer (melamine water reducer: polycarboxylate high Performance superplasticizer 1:1), 2.3 parts of ultrafine mica powder, 0.4 parts of lithium carbonate, 0.9 parts of talc.
[0024] Put the above components in a mixer and stir evenly to get cement early strength agent 1.
Embodiment 2
[0026] Weigh each component according to the following ratio: 23 parts of sodium sulfate, 5 parts of sodium nitrate, 5 parts of ferrous sulfate, 0.2 part of diethanolamine, 0.5 part of triethanolamine, 1.0 part of water reducer (melamine water reducer: polycarboxylate high Performance superplasticizer 1:1), 2.5 parts of superfine mica powder, 0.3 parts of lithium carbonate, 1.0 parts of talc powder.
[0027] Put the above components in a mixer and stir evenly to get cement early strength agent 2.
Embodiment 3
[0029] Weigh each component according to the following ratio: 27 parts of sodium sulfate, 5 parts of sodium nitrate, 3 parts of ferrous sulfate, 0.3 part of diethanolamine, 0.4 part of triethanolamine, 1.3 parts of water reducer (melamine water reducer: polycarboxylate high Performance superplasticizer 1:1), 2 parts of superfine mica powder, 0.5 parts of lithium carbonate, 0.8 parts of talc powder.
[0030] Put the above components in a mixer and stir evenly to obtain cement early strength agent 3.
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com