Method for producing soap wax and low melting point paraffin
A production method and low-melting-point technology, applied in petroleum wax recovery, petroleum wax refining, wax physical treatment, etc., can solve the problems of long production cycle and low product yield, and achieve low operating cost, low investment, and accelerated separation speed Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0041] This embodiment includes: A: emulsification and B: sweating.
[0042] A: emulsification
[0043] This part includes (A1) oil phase material preparation, (A2) water phase material preparation, (A3) emulsion preparation three steps.
[0044] (A1) Oil phase material preparation
[0045] Take Daqing crude oil Changsixian wax paste (melting point 41.5°C, oil content 13.2%) 80.0Kg, heat to 80°C and melt, add 1.5Kg of diethylene glycol monolaurate and 0.5Kg of sorbitan monolaurate, and triacetamide oleate 1.0 Kg, stir well.
[0046] (A2) Preparation of aqueous phase materials
[0047] 17.0 Kg of water was heated to 90°C.
[0048] (A3) Emulsion preparation
[0049] Stir the oil phase material at a speed of 500r / min, slowly add the water phase material prepared in (A2) to the oil phase material prepared in (A1), and continue stirring for 30min to form a water-in-oil emulsion.
[0050] B: sweating
[0051] This part includes four steps of (B1) preparation, (B2) crystalliza...
Embodiment 2
[0063] This embodiment includes: A: emulsification and B: sweating.
[0064] A: emulsification
[0065] This part includes (A1) oil phase material preparation, (A2) water phase material preparation, (A3) emulsion preparation three steps.
[0066] (A1) Oil phase material preparation
[0067] Take 80.0Kg of Daqing crude oil Changsixian wax paste (the properties are the same as in Example 1), heat to 80°C and melt, add 1.5Kg of sorbitan monostearate and 0.5Kg of lauryl betaine, and stir evenly.
[0068] (A2) Preparation of aqueous phase materials
[0069] 2.0 Kg of NaCl was dissolved in 16.0 Kg of water and heated to 90°C.
[0070] (A3) Emulsion preparation
[0071] Stir the oil phase material at a speed of 1000r / min, slowly add the water phase material prepared in (A2) to the oil phase material prepared in (A1), and continue stirring for 30min to form a water-in-oil emulsion.
[0072] B: sweating
[0073] With embodiment 1.
[0074] Properties of the target product (II) p...
Embodiment 3
[0076] This embodiment includes: A: emulsification and B: sweating.
[0077] A: emulsification
[0078] This part includes (A1) oil phase material preparation, (A2) water phase material preparation, (A3) emulsion preparation three steps.
[0079] (A1) Oil phase material preparation
[0080]Take 80.0Kg of Daqing crude oil minus second-line wax paste (melting point 50.6°C, oil content 21.4%), heat to 90°C and melt, add 2.0Kg of diethylene glycol fatty acid ester and 1.0Kg of triacetamide oleate, and stir evenly;
[0081] (A2) Preparation of aqueous phase materials
[0082] 2.0Kg of Na 2 SO 4 Dissolve in 15.0Kg of water and heat to 90°C.
[0083] (A3) Emulsion preparation
[0084] Stir the oil phase at a speed of 300r / min, slowly add the water phase material prepared in (A2) to the oil phase material prepared in (A1), and continue stirring for 20 min to form a water-in-oil emulsion.
[0085] B: sweating
[0086] This part includes four steps of (B1) preparation, (B2) crys...
PUM
Property | Measurement | Unit |
---|---|---|
melting point | aaaaa | aaaaa |
melting point | aaaaa | aaaaa |
melting point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com