Amino acid-rare earth complex high-efficiency phosphor and preparation method thereof
A technology of amino acids and phosphors, applied in the field of nanomaterials, can solve problems such as difficult large-scale industrialization and mass production, cumbersome methods and steps for synthesizing MOF, and application limitations of Ln-MOF, so as to promote application, make preparation simple, fast and convenient, Effect of improving luminous performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] ①Dissolve 0.5mmol NaOH and 2.25mmol cysteine in 10ml absolute ethanol, and stir for 10min to obtain system (1);
[0034] ② Dissolve 1.25 mmol of europium nitrate in 6 ml of water, add the solution to system (1) under stirring, and continue stirring for 10 min;
[0035] ③ After the reaction, the product was washed 4 times with absolute ethanol. After drying at 80°C for 6 hours, the novel L-cysteine-europium complex high-efficiency fluorescent powder can be obtained after cooling down.
Embodiment 2
[0037] ①Dissolve 2.25mmol KOH and 4mmol aspartic acid in 2ml absolute ethanol, and stir for 35min to obtain system (1);
[0038] ② Dissolve 2mmol of terbium nitrate in 1ml of water, add the solution into system (1) under stirring, and continue stirring for 35min;
[0039] ③ After the reaction, the product was washed 6 times with absolute ethanol. After drying at 20°C for 15 hours, a novel D-aspartic acid-terbium complex high-efficiency phosphor was obtained after cooling down.
[0040] Gained aspartic acid-terbium is combined with the high-efficiency phosphor sample to analyze with the German Bruker D8 X-ray diffractometer, and it is found that there is only one diffraction broad peak in the sample (see figure 1 ), indicating that the particle size is very small.
[0041] The sample was scanned with a scanning electron microscope S-4800 (see figure 2 ) for observation, it can be seen from the photos that the novel aspartic acid-terbium complex high-efficiency phosphor nano...
Embodiment 3
[0044] ①Dissolve 4mmol NaOH and 0.5mmol glutamic acid in 6ml absolute ethanol, and stir for 10min to obtain system (1);
[0045] ②Dissolve 0.5mmol of neodymium nitrate in 3.5ml of water, add the solution into system (1) under stirring, and continue stirring for 60min;
[0046] ③ After the reaction, the product was washed twice with absolute ethanol. After drying at 50°C for 24 hours, the novel glutamate-neodymium complex high-efficiency fluorescent powder can be obtained after cooling down.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com