Production technique of corrosion-resistant solid wood frame
A production process and anti-corrosion technology, applied in wood processing equipment, wood treatment, impregnated wood, etc., can solve problems such as poor anti-corrosion performance, achieve good gloss retention, simple process, and prolong service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A production process of a corrosion-resistant solid wood picture frame, comprising the steps of:
[0023] S1. Raw material treatment: a. Color bleaching: select wood boards without mildew marks and moths, and immerse them in 5% H2O containing 1% ammonium lignosulfonate 2 o 2 In the solution, soak for 20min;
[0024] b. Soaking: soak the selected wood in the soaking solution at 55°C, take it out after 6 hours, and then put it in the soaking solution at room temperature for another 2 hours. The soaking water level is 2cm higher than the surface of the soaked wood board;
[0025] c. Drying: Put the soaked wood into the vacuum equipment for 15 minutes, take it out, put it in the vacuum equipment, and dry it under vacuum at 85°C for 6 hours; d. Compression: Put the dried wood on the hot press Thermosetting compression treatment;
[0026] S2. Cutting: Cut the wood to the required frame according to the size measured by the picture frame, with a corner of 45°, and then sand...
Embodiment 2
[0031] A production process of a corrosion-resistant solid wood picture frame, comprising the steps of:
[0032] S1. Raw material treatment: a. Color bleaching: select wood boards without mildew marks and moths, and immerse them in 6% H2O containing 1% ammonium lignosulfonate. 2 o 2 In the solution, soak for 18min;
[0033] b. Soaking: Soak the selected wood in the soaking solution at 58°C, take it out after 6 hours, and then put it in the soaking solution at room temperature for another 2.5 hours. The soaking water level is 3cm higher than the surface of the soaked wood board;
[0034] c. Drying: Put the soaked wood into the vacuum equipment for 20 minutes, take it out, put it in the vacuum equipment, and vacuum dry it at 90°C for 6 hours; d. Compression: Put the dried wood on the hot press Thermosetting compression treatment;
[0035] S2. Cutting: Cut the wood to the required frame according to the size measured by the picture frame, with a corner of 45°, and then sand it...
Embodiment 3
[0040] A production process of a corrosion-resistant solid wood picture frame, comprising the steps of:
[0041] S1. Raw material treatment: a. Color bleaching: select wood boards without mildew marks and moths, and soak them in 7% H2O containing 1% ammonium lignosulfonate. 2 o 2 Soak in the solution for 16 minutes;
[0042] b. Soaking: Soak the selected wood in the soaking solution at 60°C, take it out after 6 hours, then put it in the soaking solution at room temperature and continue soaking for 2.5 hours, the soaking water level is 4cm higher than the soaked wood board surface;
[0043] c. Drying: Put the soaked wood into the vacuum equipment for 25 minutes, take it out, put it in the vacuum equipment, and vacuum dry it at 95°C for 6 hours; d. Compression: Put the dried wood on the hot press Thermosetting compression treatment;
[0044] S2. Cutting: Cut the wood to the required frame according to the size measured by the picture frame, with a corner of 45°, and then sand...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com