A plastic offset inspection well
An inspection well and offset technology, which is applied to water supply devices, artificial islands, underwater structures, etc., can solve the problems of inconvenience for operators to enter the inspection well and the lower part is suspended, and achieve a simple structure, low cost and high strength. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0039] Weight composition of plastic:
[0040] 95 parts of phthalic resin,
[0041] 25 parts polystyrene,
[0042] Calcium carbonate superfine powder 90 parts,
[0043] 105 pieces of glass fiber with a length of 10-15mm,
[0044] 3 parts of tert-butyl peroxy-2-ethylhexanoate,
[0045] Lubricant BYK-W966: 1 part,
[0046] Magnesium stearate 4 parts,
[0047] 2 parts of MgO powder passed through a 400-mesh sieve,
[0048] 1 part styrene,
[0049] Aluminum hydroxide superfine powder 15 parts,
[0050] 30 parts of vitrified microbead particles;
[0051] No. 58 paraffin wax 2 parts.
[0052] The measured bulk density of the vitrified microbead particles is 92kg / m 3 , the surface vitrified closed porosity rate is greater than 60%; and the vinyl silane coupling agent of 3% by weight of vitrified microbeads is pretreated in advance.
Embodiment 2
[0054] Weight composition of plastic:
[0055] 100 parts of isophthalic resin,
[0056] 28 parts of polystyrene,
[0057] Calcium carbonate superfine powder 105 parts,
[0058] 110 pieces of glass fiber with a length of 10-15mm,
[0059] 2 parts of tert-butyl peroxy-2-ethylhexanoate,
[0060]Lubricant BYK-W9010: 1 part,
[0062] 1 part of 400 mesh sieved MgO powder,
[0063] 2 parts styrene,
[0064] Aluminum hydroxide superfine powder 16 parts,
[0065] 35 parts of vitrified microbead particles;
[0066] 3 parts of No. 54 paraffin wax.
[0067] The measured bulk density of the vitrified microbead particles is 86kg / m 3 , the surface vitrified closed porosity rate is greater than 60%; and the vitrified microbead particle weight 2% vinyl silane coupling agent is pretreated in advance.
Embodiment 3
[0069] Weight composition of plastic:
[0070] 108 parts of o-phthalic resin, m-benzene resin mixture,
[0071] 30 parts polystyrene,
[0072] Calcium carbonate superfine powder 93 parts,
[0073] 120 pieces of glass fiber with a length of 10-15mm,
[0074] 2 parts of tert-butyl peroxy-2-ethylhexanoate,
[0075] Lubricant BYK-W966: 2 parts,
[0076] Magnesium stearate 2 parts,
[0077] 3 parts of MgO powder passed through a 400 mesh sieve,
[0078] 2 parts styrene,
[0079] Aluminum hydroxide superfine powder 14 parts,
[0080] 38 parts of vitrified microbead particles;
[0081] 4 parts of No. 58 paraffin wax.
[0082] The measured bulk density of the vitrified microbead particles is 95kg / m 3 , the closed cell rate of surface vitrification is greater than 60%; and pretreatment with vinyl silane coupling agent of 4% by weight of vitrified microbead particles in advance.
[0083] The processing method of three embodiments is identical:
[0084] The glass fiber is fir...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
density | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com