Method for measuring content of copper, tellurium, gold and silver in copper telluride

A method of determination, technology of copper telluride, used in measuring devices, chemical analysis by titration, instruments, etc.

Active Publication Date: 2015-07-22
YANGGU XIANGGUANG COPPER
View PDF0 Cites 11 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0007] The existing determination methods of copper in copper concentrate, tellurium in copper anode slime, tellurium in pure tellurium and gold and silver in copper concentrate have been relatively mature, while copper telluride and The composition of copper concentrate, copper anode slime and pure tellurium is quite different, and there is no determination method for gold, silver, copper and tellurium in copper telluride in the prior art

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for measuring content of copper, tellurium, gold and silver in copper telluride
  • Method for measuring content of copper, tellurium, gold and silver in copper telluride
  • Method for measuring content of copper, tellurium, gold and silver in copper telluride

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0081] Weigh 5.0034g (m 0 ) sample in a 500mL tall beaker, add a small amount of water, soak the sample, boil for a while, take it out and cool it slightly, add 15mL sulfuric acid (analytical pure), cover with a watch glass, place it on an electric heating plate to heat and dissolve, and Evaporate the solution until it emits white smoke, remove it and cool it to room temperature, rinse the surface and the salt on the wall of the cup with water, add water to the beaker to 300mL, 10mL NaCl solution (20g / L), a small amount of filter paper pulp, stir well, place in Boil on a hot plate for 5 minutes, remove and cool slightly, then filter with medium-speed filter paper. Transfer all the precipitate to filter paper, wash the precipitate with hot water until there is no blue color, and keep the filtrate (1). Put the filter paper on the glass-wiping rod and the cup wall together with the filter paper slurry loaded with the precipitate (1) into a clay crucible, put it into an assay fur...

Embodiment 2

[0118] The weight of the sample taken in this embodiment is 4.9969g, and the determination of gold, silver, copper and tellurium elements is carried out according to the measurement steps of Example 1. The measurement results and calculation process are as follows, obtained according to the following process: It contained 23.2g / t gold, 3918g / t silver, 42.33% copper and 26.62% tellurium.

[0119] Au ( g / t ) = m 4 - m 2 m 0 ;

[0120] Ag ( g / t ) = m 3 - m 4 - ...

Embodiment 3

[0142] The weight of the sample that the present embodiment takes is 5.0012g, carries out the mensuration of gold, silver, copper and tellurium element according to the mensuration step of embodiment 1, and measurement result and calculation process are as follows, obtain according to the following process: gold content is 30.5g / t at 4438g / t silver, 44.69% copper and 29.27% ​​tellurium.

[0143] Au ( g / t ) = m 4 - m 2 m 0 , Ag ( g / t ) = m 3 - m 4 - ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention provides a method for measuring the content of copper, tellurium, gold and silver in copper telluride. The method comprises the following steps: reacting a copper telluride sample and an acidic solution with a chlorine-ion-containing solution, and obtaining precipitates and a first reaction solution; performing incineration treatment on the precipitates, and obtaining incinerated residues; measuring the incinerated residues with a fire-assaying gravimetric method, and obtaining the content of gold and silver in copper telluride; reacting the first reaction solution with an alkali solution, and obtaining copper hydroxide precipitates and a second reaction solution; measuring the copper hydroxide precipitates with an iodometric method, and obtaining the content of copper in copper telluride; enabling the second reaction solution to form tellurium precipitates, measuring the tellurium precipitates with a gravimetric method, and obtaining the content of tellurium in copper telluride. The method can realize continuous separation and measurement of gold, silver, copper and tellurium in the copper telluride sample through one-time sample weighing in a process for measuring the content of copper, tellurium, gold and silver in copper telluride, so that the measurement process is simplified and the accuracy is relatively high.

Description

technical field [0001] The invention relates to the technical field of element determination, in particular to a method for determining the contents of copper, tellurium, gold and silver in copper telluride. Background technique [0002] Tellurium is a rare element, which is a silver-white crystal of orthorhombic system. High-purity tellurium is widely used as an additive in semiconductor devices, alloys, chemical raw materials, cast iron, rubber, glass and other industries due to its advantages of increasing material strength, hardness, and improving material wear and corrosion resistance. However, there are very few independent deposits of tellurium at present, which are mainly associated with the electrolytic anode slime produced in the hydrometallurgy process of non-ferrous metals such as copper, lead and zinc. [0003] Since the electrode potential of tellurium is higher than that of copper, tellurium will not be precipitated at the cathode but mainly deposited in the ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): G01N5/00G01N31/16
Inventor 姜泓李先和万双张晓天武守忠周宏鼎刘君侠沈丽
Owner YANGGU XIANGGUANG COPPER
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products