[0017] A low-odor adhesive made from the following parts by weight:
[0018] 20 parts of chlorosulfonated polyethylene, 10 parts of acrylate monomer, 20 parts of epoxy methacrylate, 10 parts of cumene hydroperoxide, 10 parts of calcium carbonate whiskers, and 10 parts of hydroquinone.
[0019] A low-odor adhesive, the preparation process of which is:
[0020] Plasticize the chlorosulfonated polyethylene on the open kneading machine, thin pass it ten times, and release the sheet for later use; in the reaction kettle, add acrylate monomer, epoxy methacrylate, and chlorosulfonated polyethylene sheet, heat Control the temperature at 40°C, stir until the chlorosulfonated polyethylene is completely dissolved, stir for 2 hours, add cumene hydrogen peroxide and stir for 20 minutes after cooling to room temperature, and finally add calcium carbonate whiskers and hydroquinone and stir until uniformly dispersed, that is Can.
Embodiment 2
[0022] A low-odor adhesive made from the following parts by weight:
[0023] 25 parts of chlorosulfonated polyethylene, 15 parts of acrylate monomer, 25 parts of epoxy methacrylate, 15 parts of cumene hydroperoxide, 15 parts of calcium carbonate whiskers, and 15 parts of hydroquinone.
[0024] A low-odor adhesive, the preparation process of which is:
[0025] Plasticize the chlorosulfonated polyethylene on the open kneading machine, thin pass it ten times, and release the sheet for later use; in the reaction kettle, add acrylate monomer, epoxy methacrylate, and chlorosulfonated polyethylene sheet, heat Control the temperature at 45°C, stir until the chlorosulfonated polyethylene is completely dissolved, stir for 3 hours, add cumene hydrogen peroxide and stir for 25 minutes after cooling to room temperature, and finally add calcium carbonate whiskers and hydroquinone and stir until uniformly dispersed, that is Can.
Embodiment 3
[0027] A low-odor adhesive made from the following parts by weight:
[0028] 30 parts of chlorosulfonated polyethylene, 20 parts of acrylate monomer, 30 parts of epoxy methacrylate, 20 parts of cumene hydroperoxide, 20 parts of calcium carbonate whiskers, and 20 parts of hydroquinone.
[0029] A low-odor adhesive, the preparation process of which is:
[0030] Plasticize the chlorosulfonated polyethylene on the open kneading machine, thin pass it ten times, and release the sheet for later use; in the reaction kettle, add acrylate monomer, epoxy methacrylate, and chlorosulfonated polyethylene sheet, heat Control the temperature at 50°C, stir until the chlorosulfonated polyethylene is completely dissolved, stir for 4 hours, add cumene hydrogen peroxide and stir for 30 minutes after cooling to room temperature, and finally add calcium carbonate whiskers and hydroquinone and stir until uniformly dispersed, that is Can.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com