Siderite-based nitrogen and phosphorus removal material and application method thereof
A simultaneous denitrification and dephosphorization, siderite technology, applied in chemical instruments and methods, other chemical processes, water/sludge/sewage treatment, etc., can solve the problems of high price and little prospect, and achieve high porosity , Strengthen the effect of chemical adsorption and effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment approach 1
[0012] Choose siderite ore, the siderite content is not less than 60%.
[0013] Crushing the siderite ore through 40 meshes;
[0014] According to the mass percentages of siderite powder, cement binder, and pulp fiber porogen are as follows: siderite powder 91%, binder 8%, porogen 1%, weigh the material, mix evenly, add the mass of the mixture Stir evenly with 25% water, use a ball forming machine to form the mixture into balls, the diameter of the ball is 3-8mm, and maintain at room temperature and 100 saturated humidity for more than 20 days;
[0015] Fill the prepared particles into the water treatment column, inoculate and enrich the nitrate-dependent iron-oxidizing bacteria culture, and the ODP value of the bacteria solution is greater than 0.2;
[0016] The volume of the bacterial solution is 2% of the volume of the experimental column, and the culture medium in the experimental column is circulated with a peristaltic pump for 5 days, and the nitrate concentration in th...
Embodiment approach 2
[0020] Choose siderite ore, the siderite content is not less than 60%, crushed through a 100-mesh sieve;
[0021] According to the following mass ratio ingredients: 83% siderite powder, 15% cement binder, 2% foaming agent and surfactant thereof, the foaming agent is such as aluminum powder, and the surfactant is alkylbenzene sulfonate salt;
[0022] Then add water with a mass ratio of 30% of the mixed material, mix evenly, shape into 4~8mm particles, and maintain at room temperature and saturated humidity for more than 20 days;
[0023] Fill the prepared particles into the water treatment column, inoculate and enrich the nitrate-dependent iron-oxidizing bacteria culture, and the ODP value of the bacteria solution is greater than 0.2;
[0024] The volume of the bacterial solution is 2% of the volume of the experimental column, and the culture solution in the experimental column is circulated with a peristaltic pump for 5 days, and the nitrate concentration in the system is mai...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com