Preparation method of environment-friendly aluminium pigment
An aluminum pigment, an environmentally friendly technology, applied in the direction of inorganic pigment treatment, chemical instruments and methods, fibrous fillers, etc., can solve the problem of not being able to export
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] A kind of preparation method of environment-friendly aluminum pigment, comprises the following steps:
[0024] a. Take 80kg of aluminum powder, 120kg of D70 solvent oil, and 2.4kg of grinding aid in parts by mass;
[0025] b. Put the configured aluminum powder, D70 solvent oil and grinding aid into a ball mill equipped with 2000kg steel balls, and grind for 22 hours to obtain a mixed slurry;
[0026] C, drop the mixed slurry obtained by grinding into a 500-order vibrating sieve for sieving and filtering;
[0027] d, put the filtered slurry into the filter press and press to obtain an aluminum slurry filter cake with 20% volatile content;
[0028] e. Put the aluminum slurry filter cake into the kneader, control the temperature in the kneader to 50°C, add the treatment agent and stir to obtain a uniform aluminum slurry with a volatile content of 26%-38%.
[0029] The limiting conditions in the above-mentioned aluminum silver paste preparation steps are as follows:
[0...
Embodiment 2
[0035] 1. A preparation method of environment-friendly aluminum pigment, comprising the following steps:
[0036] a. Take 200kg of aluminum powder, 320kg of D70 solvent oil, and 6kg of grinding aid in parts by mass;
[0037] B. Put the configured aluminum powder, D70 solvent oil and grinding aid into a ball mill equipped with 5000kg parts by mass steel balls, and grind for 23 hours to obtain a mixed slurry;
[0038] C, drop the mixed slurry obtained by grinding into a 500-order vibrating sieve for sieving and filtering;
[0039] d, put the filtered slurry into the filter press and press to obtain an aluminum slurry filter cake with 20% volatile content;
[0040] e. Put the aluminum slurry filter cake into the kneader, control the temperature in the kneader to 50°C, add the treatment agent and stir to obtain a uniform aluminum slurry with a volatile content of 26%-38%.
[0041] The limiting conditions in the above-mentioned aluminum silver paste preparation steps are as follo...
PUM
Property | Measurement | Unit |
---|---|---|
Thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction