[0011] Select the ore containing 25.30% sulfur and 2.28% arsenic, grind the raw ore through a grinding machine until the monomers are dissociated, and then enter the flotation process, and add copper smelting waste acid (including Cu 2+ The content is 0.1mg / L), the dosage is 3000g / t, 4000g / t, 5000g / t respectively, as the activator of pyrite, adjust the pH value of the pulp to 6~7, and then add 500g of arsenopyrite inhibitor sodium humate / t, collector butyl xanthate 120g / t, pine oil 100g / t for pyrite flotation to obtain sulfur concentrate.
[0012] Table 1 Sulfur concentrate flotation indicators
[0013]
Embodiment 2
[0015] Select the ore containing 25.30% sulfur and 2.28% arsenic, grind the raw ore through a grinding machine until the monomers are dissociated, and then enter the flotation process, and add copper smelting waste acid (including Cu 2+ Content selection 0.2mg / L), the dosage is 3000g / t, 4000g / t, 5000g / t respectively, as the activator of pyrite, adjust the pH value of the pulp to 6~7, and then add 500g of arsenopyrite inhibitor sodium humate / t, collector butyl xanthate 120g / t, pine oil 100g / t for pyrite flotation to obtain sulfur concentrate.
[0016] Table flotation indicators of disulfide concentrate
[0017]
Embodiment 3
[0019] Select the ore containing 25.30% sulfur and 2.28% arsenic, grind the raw ore through a grinding machine until the monomers are dissociated, and then enter the flotation process, and add copper smelting waste acid (including Cu 2+ The content is 0.3mg / L), the dosage is 3000g / t, 4000g / t, 5000g / t respectively, as the activator of pyrite, adjust the pH value of the pulp to 6~7, and then add 500g of arsenopyrite inhibitor sodium humate / t, collector butyl xanthate 120g / t, pine oil 100g / t for pyrite flotation to obtain sulfur concentrate.
[0020] Table 3 Sulfur Concentrate Flotation Index Situation
[0021]
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com