Forming process of pattern layer on surface of glass substrate
A glass substrate and surface pattern technology, which is applied in the process of producing decorative surface effects, decorative arts and other directions, can solve the problems of being susceptible to dust pollution, increase production costs, and the defective rate of finished products, so as to avoid poor process, The effect of increasing the production cost and improving the defect rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] After the glass substrate is cut to an appropriate size according to requirements, it is coated and processed. The specific process steps are:
[0024] (1) Single-color trademark pattern printing, using gravure printing equipment;
[0025] (2) UV drying, using trimercury lamp ultraviolet drying;
[0026] (3) Coating high-gloss anti-scratch topcoat, using spray coating, with a film thickness of 7 μm;
[0027] (4) drying, use a drying room, temperature 80 ℃, 30 minutes;
[0028] (5) Obtain the finished product.
Embodiment 2
[0030] After the glass substrate is cut to an appropriate size according to requirements, it is coated and processed. The specific process steps are:
[0031] (1) Coating the interface paint, using spray coating, with a film thickness of 3 μm;
[0032] (2) drying, use infrared drying, temperature 60 ℃, 20 minutes;
[0033] (3) The first layer of two-color fruit pattern printing is printed with two-color offset printing equipment;
[0034] (4) UV drying, using single iron halogen lamp ultraviolet drying;
[0035] (5) The second layer of the two-color fruit pattern printing layer is printed using two-color offset printing equipment;
[0036] (6) UV drying, using a mercury lamp-iron halogen lamp ultraviolet drying;
[0037] (7) Coating high-gloss and stain-resistant topcoat, using spray coating, with a film thickness of 6 μm;
[0038] (8) drying, use infrared drying, temperature 80 ℃, 30 minutes;
[0039] (9) Obtain the finished product.
Embodiment 3
[0041] After the glass substrate is cut to an appropriate size according to requirements, it is coated and processed. The specific process steps are:
[0042] (1) Coating the interface paint, using spray coating, the film thickness is 2 μm;
[0043] (2) UV drying, using double mercury lamp ultraviolet drying;
[0044] (3) Coating mending soil, using roller coating, with a film thickness of 7 μm;
[0045] (4) UV drying, using double mercury lamp ultraviolet drying;
[0046] (5) Apply colored paint, use spraying, film thickness 5 μm;
[0047] (6) UV drying, using double mercury lamp ultraviolet drying;
[0048] (7) The first layer of three-color artistic character pattern printing is printed by roller-type three-color pad printing equipment;
[0049] (8) UV drying, using single iron halogen lamp ultraviolet drying;
[0050] (9) The second layer of three-color artistic character pattern printing is printed by roller-type three-color pad printing equipment;
[0051] (10) UV ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com