Method for preparing light-permeable stereo ceramic product with slightly-embossed carving process and application thereof
A technology for ceramic products and processes, which is applied in the field of preparation of light-transmitting three-dimensional ceramic products by the hidden carving process, can solve the problems of poor light-transmitting performance of products, increase product breakage rate, affect product yield, etc. Low production cost and strong stereoscopic effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Embodiment 1: a preparation method of a hemispherical candle cover, the process steps of which include:
[0018] (1) To make porcelain mud, mix the porcelain mud with water and sodium silicate as usual, and stir to form a slurry;
[0019] (2) Make a hemispherical candle cover mold, and use the hidden carving method to carve the desired pattern on the mold, that is, use the method of embossing, sinking carving, shadow carving and anti-carving.
[0020] (3) Pour the mud on the designed hemispherical candle cover mold;
[0021] (4) Dry bath for 40 minutes, demould to obtain ceramic embryo;
[0022] (5) Body trimming to remove excess mold lines and sundries;
[0023] (6) Firing, the firing temperature of the product is 1250°C, and the firing time is 10 hours.
[0024] That is, a light-transmitting hemispherical candle cover with a three-dimensional pattern is obtained.
[0025] The rest are operated according to the conventional technological process.
Embodiment 2
[0026] Embodiment 2: a preparation method of a cylindrical table lamp, the process steps include:
[0027] (2) To make a cylindrical table lamp mold, use the hidden carving method to engrave the desired pattern on the mold, that is, to use the method of combining relief carving, sink carving, shadow carving and anti-carving method;
[0028] (3) Pour the mud on the designed cylindrical lamp mold;
[0029] (6) Firing, the firing temperature of the product is 1280°C, and the firing time is 9 hours;
[0030] Steps (1), (4), (5) are the same as in Example 1.
[0031] That is, a cylindrical table lamp that transmits light and has a three-dimensional pattern is obtained.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com