A technique for latex gloves and a production method, which is applied in the field of flocking latex gloves and its production, and can solve the problem of high latex content, gelation time, high quality of fluff, poor cooling effect of sprayed latex gloves, and restrictions on the use of latex gloves And other problems, to achieve the effect of not easy hair removal, good demoulding effect and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0048] A flocking latex glove, its production method comprises the following processing steps:
[0049] (1) Mold preparation:
[0050] Soak the glove mold in a 5% nitric acid solution at 20°C for 3 minutes, then soak it in a 5% sodium carbonate solution at 20°C for 4 minutes, and finally spray it with clean water Clean until neutral; hang the mold and dry it with hot air at 50°C;
[0051] Slowly add 5 parts by weight of common starch and 25 parts by weight of calcium chloride into 260 parts by weight of water under stirring, and react for 0.5 hours at a temperature of 50°C to prepare a coagulant;
[0052] Dip the cleaned and dried glove mold into a coagulant and dry it;
[0053] (2) Dip latex for the first time:
[0054] Add 60 parts by weight of natural latex and 3 parts by weight of neoprene latex into the reactor under stirring, and after stirring for 0.5 hours, slowly add 5 parts by weight of deionized water and 0.5 parts by weight of sulfur , 0.5 parts by weight of ZD...
Embodiment 2
[0070] A flocking latex glove, its production method comprises the following processing steps:
[0071] (1) Mold preparation:
[0072] Soak the glove mold in a sulfuric acid solution with a concentration of 2% by weight at 40°C for 10 minutes, then soak it in a sodium hydroxide solution with a concentration of 2% by weight at 40°C for 5 minutes, and finally spray it with clean water Rinse and wash until neutral; hang the mold and dry it with hot air at 80°C;
[0073] Slowly add 40 parts by weight of ordinary starch and 40 parts by weight of calcium nitrate to 470 parts by weight of water under stirring, and keep the temperature at 100°C for 2 hours to prepare the coagulant;
[0074] Dip the cleaned and dried glove mold into a coagulant and dry it;
[0075] (2) Dip latex for the first time:
[0076] Add 110 parts by weight of 60% natural latex and 20 parts by weight of neoprene latex into the reactor under stirring. After stirring for 2 hours, slowly add 30 parts by weight o...
Embodiment 3
[0092] A flocking latex glove, its production method comprises the following processing steps:
[0093] (1) Mold preparation:
[0094] Put the glove mold into the hydrochloric acid solution with a concentration of 3% by weight at 30°C for 6 minutes, then soak it in a solution of potassium hydroxide with a concentration of 4% by weight at 30°C for 3 minutes, and finally spray it with water Rinse and wash until neutral; hang the mold and dry it with hot air at 25°C;
[0095] Slowly add 20 parts by weight of common starch and 32 parts by weight of calcium sulfate into 350 parts by weight of water under stirring, and react for 1 hour at a temperature of 70°C to prepare the coagulant;
[0096] Dip the cleaned and dried glove mold into a coagulant and dry it;
[0097] (2) Dip latex for the first time:
[0098] Add 85 parts by weight of 60% natural latex and 12 parts by weight of chloroprene latex into the reactor under stirring. After stirring for 1 hour, slowly add 18 parts by w...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
length | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com