[0026] Example 1 Preparation of Calcium Phosphate Bone Cement Loaded with Lysostaphin
[0027] 1) Preparation of sodium alginate-lysostaphin complex suspension
[0028] Take 0.1 g of lysostaphin and dissolve in 1 ml of water. Another 0.1 g of sodium alginate was dissolved in 10 ml of water. Mix and stir 1ml of lysostaphin solution and 1ml of sodium alginate solution to obtain sodium alginate-lysostaphin complex suspension.
[0029] 2) Preparation of calcium phosphate cement
[0030] Mix 57mg of tricalcium phosphate and 43mg of calcium hydrogen phosphate powder evenly, add 30μl of calcium chloride aqueous solution (10%), reconcile and stir evenly, put the resulting paste in a mold, and after demoulding, place it at 37°C, 100% Fully solidified for 24 hours under relative humidity to obtain calcium phosphate bone cement.
[0031] 3) Preparation of calcium phosphate bone cement loaded with lysostaphin
[0032] Soak the calcium phosphate bone cement obtained in step 2) into th...
Embodiment 2
[0033] Embodiment 2 Preparation of calcium phosphate bone cement loaded with lysozyme
[0034] 1) Preparation of sodium alginate-lysozyme complex suspension Take 0.1 g of lysozyme and add 1 ml of water to dissolve it. Another 0.1 g of sodium alginate was dissolved in 10 ml of water. Mix and stir 1ml of lysostaphin solution and 1ml of sodium alginate solution to obtain sodium alginate-lysozyme complex suspension.
[0035] 2) Preparation of porous calcium phosphate cement
[0036] Mix 57mg of tricalcium phosphate, 43mg of calcium hydrogen phosphate powder and 10mg of solid paraffin (through a 40-mesh sieve), and add 30 μl of calcium chloride aqueous solution (10%), mix and stir evenly, place the resulting paste in a mold, and remove After molding, place it at 37°C and 100% relative humidity for full curing for 24 hours, put it in absolute ethanol for 12 hours at 70°C, change the absolute ethanol constantly, take it out and dry it in an oven to obtain porous calcium phosphate b...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com