A kind of copper red glaze and its production method and the method for making ceramic product with it
A production method, the technology of copper red glaze, applied in the field of ceramics, can solve the problems of burning loss, smoking, pinhole defects, etc., and achieve the effects of avoiding glaze flow, high yield and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Example 1: Prepare the following components in proportion: 26 parts by weight of quartz, 30 parts by weight of feldspar, 12 parts by weight of limestone, 14 parts by weight of barium carbonate, 6 parts by weight of clay, 3 parts by weight of zinc oxide, 3 parts by weight of borax; Mix the above components and add water ball milling to form a glaze slurry with a solid particle fineness of passing a 200-mesh sieve;
[0017] Prepare the following components in proportion: 1.2 parts by weight of copper oxide, 0.8 parts by weight of iron trioxide, 2 parts by weight of tin dioxide, and 2 parts by weight of lead oxide; use a small ball mill and water ball mill to form a solid particle with a fineness of 325 mesh Screened slurry
[0018] Mix the glaze slurry and the slurry evenly to make a copper red glaze slurry.
[0019] Take a batch of green ceramic vases, clean them up, apply the above-mentioned glaze slurry on the ceramics body by dipping the glaze, and control the thickness of ...
Embodiment 2
[0022] Example 2: Prepare the following components in proportion: 30 parts by weight of quartz, 26 parts by weight of feldspar, 12 parts by weight of limestone, 14 parts by weight of barium carbonate, 8 parts by weight of clay, 2 parts by weight of zinc oxide, 2 parts by weight of borax; Mix the above components and add water ball milling to form a glaze slurry with a solid particle fineness of passing a 200-mesh sieve;
[0023] Prepare the following components in proportion: 2 parts by weight of copper carbonate, 0.8 parts by weight of iron trioxide, 1.2 parts by weight of tin dioxide, and 2 parts by weight of lead oxide; use a small ball mill with water ball mill to form a solid particle with a fineness of 325 mesh Screened slurry
[0024] Mix the glaze slurry and the slurry evenly to make a copper red glaze slurry.
[0025] Take a batch of ceramic figure sculpture biscuits, clean them up, and apply the above-mentioned glaze slurry to the parts that need decoration, and the thickn...
Embodiment 3
[0028] Example 3: Prepare the following components in proportions: 32 parts by weight of quartz, 28 parts by weight of feldspar, 12 parts by weight of limestone, 14 parts by weight of barium carbonate, 8 parts by weight of clay, and 2 parts by weight of zinc oxide; mix the above components, Add water ball mill to form a glaze slurry with a solid particle fineness that passes through a 300-mesh sieve;
[0029] Prepare the following components in proportion: 1.6 parts by weight of copper oxide, 0.8 parts by weight of ferric oxide, and 2.2 parts by weight of tin dioxide; use a small ball mill with water ball mill to form a slurry with a solid particle size that passes through a 325 mesh sieve;
[0030] Mix the glaze slurry and the slurry evenly to make a copper red glaze slurry.
[0031] Take a batch of green ceramic discs, clean them up, and apply the above-mentioned glaze slurry on the ceramic discs by glazing, and control the thickness of the glaze layer to 1.4mm;
[0032] After dryin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com