[0016] According to the present invention, the preparation method of the silica-alumina zeolite molecular sieve through metal-modified MFI structure and / or MEL structure comprises the following steps:
[0017] (1) The zeolite molecular sieve raw powder is subjected to NH 4+ Ion exchange and roasting to prepare acidic zeolite molecular sieves;
[0018] (2) Use soluble non-rare earth metal salt solution and / or soluble rare earth metal salt solution to impregnate acidic zeolite molecular sieve, as long as the impregnation time and the concentration of metal salt in soluble non-rare earth metal salt solution and / or soluble rare earth metal salt solution meet The content of the metal component in the catalyst is sufficient; after drying and roasting, a non-rare earth metal and / or rare earth metal modified zeolite molecular sieve is obtained;
[0019] (3) The modified catalyst prepared in the step (2) is pressed into tablets, dried and shaped.
[0020] Wherein, in step (1), the ra...
Embodiment 1
[0024] This example is used to illustrate the preparation of fixed bed catalyst
[0025] (1) 500 grams of ZSM-5 zeolite molecular sieve former powder (Nankai University Catalyst Factory) SiO 2 / Al 2 o 3 =50 (molar ratio) roasting at 550°C to remove template agent, exchange 4 times with 0.5 molar equivalent ammonium nitrate solution in 80°C water bath, dry at 120°C air after exchange, and roast at 550°C for 3 hours to obtain HZSM-5 zeolite molecular sieve.
[0026] (2) 20 grams of HZSM-5 zeolite molecular sieves prepared in step (1) were pressed into tablets, and the 40-60 mesh samples were obtained after crushing and screening, which were divided into two parts. 3% by weight and 9% by weight of zinc nitrate Zn (NO3 ) 2 The solution was soaked for 4 hours, dried at 120°C, and roasted in air at 550°C for 6 hours to obtain a non-rare earth metal modified catalyst;
[0027] (3) With a concentration of 10% by weight La(NO 3 ) 3 The aqueous solution impregnation step (2) obta...
Embodiment 2
[0029] This example is used to illustrate the preparation of fixed bed catalyst
[0030] (1) 500 grams of ZSM-5 zeolite molecular sieve former powder (Nankai University Catalyst Factory) (SiO 2 / Al 2 o 3 =50) Roast at 550°C to remove template agent, exchange 4 times with 0.5 molar equivalent ammonium nitrate solution in 80°C water bath, dry in air at 120°C after exchange, and roast at 550°C for 3 hours to obtain HZSM-5 Zeolite molecular sieve.
[0031] (2) 20 grams of HZSM-5 zeolite molecular sieves prepared in step (1) were pressed into tablets, and the 40-60 mesh samples were obtained after crushing and screening, which were divided into two parts. 3.7% by weight and 11.1% by weight of molybdenum nitrate Mo (NO 3 ) 3 The solution was soaked at room temperature for 4 hours, dried at 120°C, and then calcined in air at 550°C for 6 hours to obtain a non-rare earth metal modified catalyst;
[0032] (3) With a concentration of 10% by weight La(NO 3 ) 3 The aqueous solution...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com