Water soluble low-temperature-solidification appliance insulating varnish and preparation method thereof
An insulating varnish, water-soluble technology, applied in the direction of coating, etc., can solve the problems of not being able to withstand the baking temperature above 100 ℃, high baking and curing temperature, multi-energy, etc., to achieve energy saving, strong paint film adhesion, The effect of improving the performance of the paint film
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0041] Embodiment 1: formula composition is as follows:
[0042] 1. Ethyl acrylate 35.0kg
[0043] 2. Silicone resin 15.0kg
[0044] 3. Diethylene glycol 4.0kg
[0045] 4. Diethanolamine 1.0kg
[0046] 5. Benzoyl peroxide 0.5kg
[0047] 6. Amino resin INEOS747 3.0kg
[0048] 7. Silicone oil 0.4kg
[0049] 8. BYK028 0.2kg
[0050] 9. Deionized water 40.9kg
[0051] Stir slowly at room temperature, mix the components ethyl acrylate, silicone resin, diethylene glycol, benzoyl peroxide and 50% deionized water evenly, and stir for about 20 minutes; then add BYK028, amino resin INEOS747 in sequence , silicone oil and the remaining deionized water, and continue to stir for 20 minutes; then slowly add diethanolamine dropwise, adjust the pH to the range of 8.0-9.0, and the finished product can be obtained. It can be used as impregnating insulating varnish for transformers, micro-motors, coils, etc. The temperature of baking and curing film formation is 80-90°C, and the baking t...
Embodiment 2
[0053] The preparation process is the same as in Example 1, but the material and content of each component change to as follows:
[0054] 1. Octyl acrylate 32.0kg
[0055] 2. Silicone resin 10.0kg
[0056] 3. Ethylene glycol 6.0kg
[0057] 4. Monoethanolamine 1.2kg
[0058] 5. Benzoyl peroxide 1.0kg
[0059] 6. Amino resin INEOS747 3.5kg
[0060] 7. Polyether modified silicone oil 0.6kg
[0061] 8. BYK028 0.30kg
[0062] 9. Deionized water 45.4kg
[0063] The preparation process is the same as in Example 1.
Embodiment 3
[0065] The preparation process is the same as in Example 1, but the material and content of each component change to as follows:
[0066] 1. Butyl acrylate 38.0kg
[0067] 2. Silicone resin 12.0kg
[0068] 3. Glycerol 5.0kg
[0069] 4. Triethanolamine 1.0kg
[0070] 5. Benzoyl peroxide 0.8kg
[0071] 6. Amino resin INEOS747 2.5kg
[0072] 7. Silicone oil 0.5kg
[0073] 8. BYK347 0.35kg
[0074] 9. Deionized water 40.00kg
[0075] The change of each component is mainly adjusted according to the actual demand of different electrical products and the change of common components in order to obtain the best comprehensive performance.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com