Bamboo charcoal-polyvinyl formal biological carrier and preparation thereof
A polyvinyl formal, biological carrier technology, applied in sustainable biological treatment, biological water/sewage treatment, water/sludge/sewage treatment, etc., can solve the problems of difficult cleaning and replacement, high price and high wear rate , to achieve the effect of favorable film hanging, strong adsorption and high strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] (1) Measure 80 parts of water, weigh 0.2 part of sodium hydroxide, take an appropriate amount of water from the measured water, and dissolve the sodium hydroxide for use.
[0030] (2) Heat the remaining water to 70°C, add 10 parts of polyvinyl alcohol and stir, and control the temperature at 90-95°C until the polyvinyl alcohol is completely dissolved.
[0031] (3) Add 0.5 part of hydrochloric acid, take 5 parts of 36% formaldehyde solution and slowly add to (2) within 30 minutes, keep the temperature at 75-95° C., and stir.
[0032] (4) When a flocculent precipitate appears in the solution (3), add an appropriate amount of ethanol dropwise until the precipitate disappears, continue stirring and heating, and when the flocculent precipitate appears again, add an appropriate amount of ethanol dropwise until the precipitate disappears.
[0033] (5) After reacting for 40-60 minutes, cool down to 50°C, add sodium hydroxide, and adjust the pH value to 8-9.
[0034] (6) Add 20...
Embodiment 2
[0039] (1)-(5) are the same as in Example 1.
[0040] (6) Add 30 parts of bamboo charcoal into (5), and stir well.
[0041] (7) Add 6 parts of calcium carbonate into (6) and stir evenly.
[0042] (8) Add 4 parts of citric acid into (7) and stir evenly, pour into the mold and let it stand for foaming.
[0043] (9) Wash and cut the product after foaming is complete.
Embodiment 3
[0045] (1)-(5) are the same as in Example 1.
[0046] (6) Add 25 parts of bamboo charcoal into (5), and stir well.
[0047] (7) Add 9 parts of calcium carbonate into (6) and stir evenly.
[0048] (8) Add 6 parts of citric acid into (7) and stir evenly, then pour into the mold and let stand to foam.
[0049] (9) Wash and cut the product after foaming is complete.
PUM
Property | Measurement | Unit |
---|---|---|
specific surface area | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com