A phosphate Fe, lithium and aluminum shell column battery and its making technology
A technology of lithium iron phosphate and cylindrical batteries, which is applied in the manufacture of electrolyte batteries, secondary batteries, battery electrodes, etc., and can solve the problems of difficulty in coating positive electrode slurry, low capacity, and difficult processing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0104] Embodiment 1 (preferred embodiment):
[0105] The weight percent proportioning of positive electrode slurry:
[0106] Cathode material: 88.5%;
[0107] Superconducting carbon black: 3%;
[0108] Conductive graphite: 1.5%;
[0109] Polyvinylidene fluoride: 7%;
[0110] The weight percent proportioning of negative electrode slurry:
[0111] Negative electrode material: 94.4%;
[0112] Superconducting carbon black: 1%;
[0113] Sodium carboxymethylcellulose: 1.8%;
[0114] Solid content of styrene-butadiene rubber emulsion: 2.8%.
[0115] Embodiment 1 is the best embodiment, which has good electrical conductivity, good adhesion, and can be discharged with high power.
Embodiment 2
[0117] The weight percent proportioning of positive electrode slurry:
[0118] Cathode material: 87%;
[0119] Superconducting carbon black: 4%;
[0120] Conductive graphite: 2%;
[0121] Polyvinylidene fluoride: 7%;
[0122] The weight percent proportioning of negative electrode slurry:
[0123] Negative electrode material: 94.4%;
[0124] Superconducting carbon black: 0.5%;
[0125] Conductive graphite: 0.5%;
[0126] Sodium carboxymethylcellulose: 1.8%;
[0127] Solid content of styrene-butadiene rubber emulsion: 2.8%.
[0128] Example 2 has better conductivity and can be discharged with high power.
Embodiment 3
[0130] The weight percent proportioning of positive electrode slurry:
[0131] Cathode material: 86%;
[0132] Superconducting carbon black: 4.7%;
[0133] Conductive graphite: 2.3%;
[0134] Polyvinylidene fluoride: 7%;
[0135] The weight percent proportioning of negative electrode slurry:
[0136] Anode material: 96%;
[0137] Sodium carboxymethylcellulose: 1.4%;
[0138] Solid content of styrene-butadiene rubber emulsion: 2.6%.
[0139] Example 3 has better electrical conductivity, high negative electrode capacity, and is suitable for high-power discharge.
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
height | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com