Polymer power cell anode-cathode film
A cathode and anode, polymer technology, applied in the direction of battery electrodes, active material electrodes, organic electrolyte batteries, etc., can solve the problems of waste of raw materials, large thickness deviation of battery cathode and anode film, high yield, etc., to improve fluidity, The effect of convenient process operation and small thickness deviation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] battery anode film
[0022] Natural graphite 2250g
[0023] Super P 60g
[0024] Dibutyl phthalate 240g
[0025] Vinylidene fluoride-hexafluoropropylene-A 45g
[0026] Vinylidene fluoride-hexafluoropropylene-B 405g
[0027] Acetone 3900g
[0028] The production process of the present invention is as follows: add the required anode material, conductive agent, and binder into the mixer, fully mix, then add the solvent, stir evenly, and make the anode slurry, and then use the anode slurry made Coating on a cloth machine and then drying on a polyester film at 20°C to 80°C to obtain an anode film.
[0029] battery cathode film
[0030] Lithium manganate 2250g
[0031] Super P 150g
[0032] Dibutyl phthalate 450g
[0033] Vinylidene fluoride-hexafluoropropylene-A 15g
[0034] Vinylidene fluoride-hexafluoropropylene-B 145g
[0035] Acetone 2200g
[0036] The production process of the present invention is as follows: add the required cathode material, conductive age...
Embodiment 2
[0038] battery anode film
[0039] Natural graphite 2400g
[0040] Super P 30g
[0041] Dibutyl phthalate 240g
[0042] Vinylidene fluoride-hexafluoropropylene-A 297g
[0043] Vinylidene fluoride-hexafluoropropylene-B 33g
[0044] Acetone 3200g
[0045] The production process of the present invention is as follows: add the required anode material, conductive agent, and binder into the mixer, fully mix, then add the solvent, stir evenly, and make the anode slurry, and then use the anode slurry made Coating on a cloth machine and then drying on a polyester film at 20°C to 80°C to obtain an anode film.
[0046] battery cathode film
[0047] Lithium manganate 2400g
[0048] Super P 120g
[0049] Dibutyl phthalate 240g
[0050] Vinylidene fluoride-hexafluoropropylene-A 216g
[0051] Vinylidene fluoride-hexafluoropropylene-B 24g
[0052] Acetone 2700g
[0053] The production process of the present invention is as follows: add the required cathode material, conductive age...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com