[0025] 1. Preparation:
[0026] Dye: Astrachong Red 0.15% Auxiliary: 0.4g / L Glacial Acetic Acid
[0027] Asquila Chonglan 0.25% 3.0g / L Yuan Ming Powder
[0028] Astra Chong Black 5.00%
[0029] Bath ratio: 1:25.
[0030] 2. Dyeing
[0031] Pine the bamboo charcoal modified polyester fiber tops and place them in a high-temperature wool top dyeing machine, run at 40°C for 5 minutes, add 0.4g / L glacial acetic acid, 3g / L sodium sulfate, run for 5 minutes, add dyes, and start to heat up after 10 minutes of operation , the heating rate is 1.5°C / min. When the temperature reaches 80°C, stop heating and keep warm for 15 minutes, then raise the temperature to 110°C at a rate of 1°C / min, and run for 60 minutes to drain and rinse directly.
[0032] 3. Post-processing
[0033] The dyed bamboo charcoal modified polyester fiber tops are first placed in a bath composed of 2g / L caustic soda, 2g / L hydrosulfite, and 1g / L nonionic surfactant, treated at 80°C for 30min, and then p...
Embodiment 2
[0035] 1. Preparation:
[0036] Dye: Astrachong Red 0.1% Auxiliary: 0.4g / L Glacial Acetic Acid
[0037] Asquila Chongjinhuang 0.2% 2.5g / L Yuan Ming Powder
[0038] Asquila Chonglan 0.05%
[0039] Bath ratio: 1:25.
[0040] 2. Dyeing
[0041] Pine the bamboo charcoal modified polyester fiber tops and place them in a high-temperature wool top dyeing machine, run at 40°C for 5 minutes, add 0.4g / L glacial acetic acid, 2.5g / L sodium sulfate, run for 5 minutes, add dyes, and start after 10 minutes of operation Heating, the heating rate is 1.5°C / min. When the temperature reaches 80°C, stop heating and keep warm for 10 minutes, then raise the temperature to 110°C at a rate of 1°C / min, and run for 40 minutes to drain and rinse directly.
[0042] 3. Post-processing
[0043] Place the dyed bamboo charcoal modified polyester fiber in 3% (fabric weight percentage) soaping solution, and treat it at 90°C for 20min.
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com