Glass beer bottle and preparation method thereof
A beer bottle and glass technology, applied in glass manufacturing equipment, glass molding, manufacturing tools and other directions, can solve the problems of poor crack resistance, glass bottles are easily broken, affecting the production of beer, etc., and achieve high product quality. , The production conditions are easy to control, and the effect of improving chemical stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] A glass beer bottle, the formula of the glass beer bottle includes the following components in parts by weight: 30 parts of glass slag, 30 parts of quartz sand, 10 parts of soda ash, 5 parts of calcite, and 5 parts of feldspar , 1 part of calcium phosphate, 1 part of manganese dioxide.
[0025] The preparation method specifically comprises the following steps:
[0026] Step 1: Weigh glass slag, quartz sand, soda ash, calcite, feldspar, calcium phosphate, manganese dioxide in proportion, and set aside;
[0027] Step 2: Put the raw material components weighed in step 1 together into a pulverizer to pulverize and mix evenly to obtain powdery raw materials;
[0028] Step 3: sending the pulverized raw materials into a dryer for drying treatment and then ball milling to obtain ball mill powder;
[0029] Step 4: send the ball mill powder to the melting furnace, and heat at high temperature to obtain a uniform and bubble-free glass stock solution. The temperature of high temp...
Embodiment 2
[0033] A glass beer bottle, the formula of the glass beer bottle includes the following components in parts by weight: 40 parts of glass slag, 35 parts of quartz sand, 15 parts of soda ash, 15 parts of calcite, and 15 parts of feldspar , 3 parts of calcium phosphate, 3 parts of manganese dioxide.
[0034] The preparation method specifically comprises the following steps:
[0035] Step 1: Weigh glass slag, quartz sand, soda ash, calcite, feldspar, calcium phosphate, manganese dioxide in proportion, and set aside;
[0036] Step 2: Put the raw material components weighed in step 1 together into a pulverizer to pulverize and mix evenly to obtain powdery raw materials;
[0037] Step 3: sending the pulverized raw materials into a dryer for drying treatment and then ball milling to obtain ball mill powder;
[0038] Step 4: send the ball mill powder to the melting furnace, and heat at high temperature to obtain a uniform glass stock solution without bubbles. The temperature of high ...
Embodiment 3
[0042] A glass beer bottle, the formula of the glass beer bottle includes the following components in parts by weight: 33 parts of glass slag, 32 parts of quartz sand, 12 parts of soda ash, 8 parts of calcite, and 8 parts of feldspar , 1.5 parts of calcium phosphate, 1.5 parts of manganese dioxide.
[0043] The preparation method specifically comprises the following steps:
[0044] Step 1: Weigh glass slag, quartz sand, soda ash, calcite, feldspar, calcium phosphate, manganese dioxide in proportion, and set aside;
[0045] Step 2: Put the raw material components weighed in step 1 together into a pulverizer to pulverize and mix evenly to obtain powdery raw materials;
[0046] Step 3: sending the pulverized raw materials into a dryer for drying treatment and then ball milling to obtain ball mill powder;
[0047] Step 4: send the ball mill powder to the melting furnace, and heat at high temperature to obtain a uniform and bubble-free glass stock solution. The temperature of hig...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com