Novel high polymer peristaltic grouting material and manufacturing process thereof
A technology of grouting materials and high polymers, which is applied in the direction of building insulation materials, building structures, building components, etc., and can solve performance defects such as inability to adapt to requirements, elastic-plastic properties, self-healing properties, bonding properties, and aging resistance. problems, to achieve the effect of improving waterproof effect, excellent water repellency, and excellent adaptability to the base layer
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] In this example, the new polymer peristaltic grouting material consists of 18% asphalt, 18% naphthenic oil, 9% styrene, 8% styrene-butadiene rubber, and 5% crosslinking agent in terms of mass percentage. , 3% high temperature antioxidant, 8% machine sand, 9% soft calcium are mixed.
[0029] The manufacturing process steps are as follows:
[0030] (1) After putting 18% asphalt into an electric boiler and heating to 130°C, stir for 10-30 minutes;
[0031] (2) Weigh 18% naphthenic oil, add it to the bitumen obtained in step (1) at 130°C, control the temperature to 130°C, start stirring at a low speed, and stir for 0.5 hours;
[0032] (3) Warm up the mixture obtained in step (2) to 160° C., then add 9% styrene and 8% styrene-butadiene rubber, put them into a colloid mill together, stir and circulate, shear and grind for 1 hour until there are no visible particles;
[0033] (4) Add 8% machine sand and 9% soft calcium to step (3), and continue stirring for 1 hour; keep at 1...
Embodiment 2
[0037] In this example, the new polymer peristaltic grouting material consists of 25% asphalt, 25% naphthenic oil, 13% styrene, 12% styrene-butadiene rubber, and 8% crosslinking agent in terms of mass percentage. , 6% high temperature antioxidant, 12% machine sand, 14% soft calcium are mixed.
[0038] The manufacturing process steps are as follows:
[0039] (1) Put 25% asphalt into an electric boiler and heat it to 160°C, then stir for 30 minutes;
[0040] (2) Weigh 25% naphthenic oil, add it to the bitumen obtained in step (1) at 160°C, control the temperature to 160°C, start stirring at a low speed, and stir for 1 hour;
[0041] (3) Warm up the mixture obtained in step (2) to 190°C, then add 13% styrene and 12% styrene-butadiene rubber, put them into a colloid mill together, stir and circulate, shear and grind for 2 hours until there are no visible particles;
[0042] (4) Add 12% machine sand and 14% soft calcium to step (3), continue stirring for 1.5 hours; keep at 190°C;...
Embodiment 3
[0046] In this example, the new polymer peristaltic grouting material consists of 23% asphalt, 23% naphthenic oil, 11% styrene, 12% styrene-butadiene rubber, and 7% crosslinking agent in terms of mass percentage. , 4% high-temperature antioxidant, 9% machine sand, and 11% soft calcium are mixed.
[0047] The manufacturing process steps are as follows:
[0048] (1) Put 23% asphalt into an electric boiler and heat it to 160°C, then stir for 30 minutes;
[0049] (2) Weigh 23% naphthenic oil, add it to the bitumen obtained in step (1) at 160°C, control the temperature to 160°C, start stirring at a low speed, and stir for 1 hour;
[0050] (3) Warm up the mixture obtained in step (2) to 190°C, then add 11% styrene and 12% styrene-butadiene rubber, put them into a colloid mill together, stir and circulate, shear and grind for 2 hours until there are no visible particles;
[0051] (4) Add 9% machine sand and 11% soft calcium to step (3), continue stirring for 1.5 hours; keep at 190°...
PUM
Property | Measurement | Unit |
---|---|---|
whiteness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com