Iron-substituted tungsten phosphorus polyacid polydopamine nano mimic enzyme as well as preparation method and application thereof
A dopamine nano and enzyme-mimicking technology, applied in the field of nanotechnology and catalytic materials, can solve problems such as analysis and inability to other biological substances
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0110] Embodiment 1 Synthesis of iron-substituted tungstophosphopolyacid polydopamine nanozyme of the present invention
[0111] 1) Preparation of precursor Na 8 [HPW 9 o 34 ]
[0112] Weigh 120g of sodium tungstate dihydrate and dissolve it in 150mL of water at 100°C, add 3mL of concentrated phosphoric acid to it under stirring, and then add 22mL of glacial acetic acid dropwise under vigorous stirring. This operation is completed within 30min, and a white precipitate Gradually appear, then filter, stir and wash the precipitate in 250mL 4mol / L NaCl solution, filter again, and dry at high temperature to obtain the desired substance NaCl 8 [HPW 9 o 34 ].
[0113] 2) Preparation of K 10 P 2 W 18 Fe 4 (H 2 O) 2 o 68
[0114]Dissolve 1.5 mmol of ferric chloride or ferric nitrate in 10 mL of water, and add 0.75 mmol of solid Na to the solution 8 [HPW 9 o 34 ], stir, mix and heat the two to homogeneous phase, filter the precipitate while it is hot, add 5g of solid po...
Embodiment 2
[0119] Example 2 Experiment of iron-substituted tungstophosphopolyacid polydopamine nano-mimetic enzyme catalyzing hydrogen peroxide oxidation of its substrate
Embodiment 2A
[0120] Example 2A Experiment of iron-substituted tungstophosphopolyacid polydopamine nano-mimetic enzyme catalyzing hydrogen peroxide oxidation of o-phenylenediamine (OPD)
[0121] (1) Take 800μL, 0.1M, pH4 phosphate buffer solution, add 500μL, 0.9mM o-phenylenediamine (OPD), 500μL, 250mM H 2 o 2 and 200 μL 25 μg / ml iron-substituted tungstophosphopolyacid polydopamine nano-mimetic enzyme, and then mix the above solution evenly; react at room temperature for 10 minutes.
[0122] (2) Measure above-mentioned mixed solution with ultraviolet-visible absorption spectrophotometer and measure ultraviolet absorption spectrum at 350-700nm respectively, experimental result is as follows image 3 (a) shown. Measure the emission spectrum at 450-700nm with a fluorescence spectrophotometer, and the experimental results are as follows image 3 (b) shown.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com