Water-based propylene marker pen ink and preparation method thereof
An acrylic marker, pen ink technology, applied in the direction of ink, household appliances, applications, etc., can solve problems such as user influence, and achieve the effect of good opacity, strong biological safety, and optimal whiteness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] A white water-based acrylic marker ink consisting of the following components by weight:
[0025] Ningbo Xinfu titanium dioxide 10.0%, polyethylene glycol 1.5%, polyvinyl alcohol 1.5%, ammonium polyacrylate 2.0%, nonylphenol polyoxyethylene ether 2.0%, BASF Zhuangqiao acrylic resin emulsion 50.0%, purified water 33 %, total weight 100 grams.
[0026] The preparation method of above white water-based acrylic marker pen ink, comprises the following steps:
[0027] ① Weigh each component according to the above weight and proportion, the total weight is 100 grams;
[0028] ②Mix the Ningbo Xinfu titanium dioxide weighed in step ① with pure water, and ultrasonically treat it for 30 minutes to obtain a water-dispersed mixture of titanium dioxide;
[0029] ③ Add the polyethylene glycol and polyvinyl alcohol weighed in step ① to the mixture 1 obtained in step ②, stir at 80 degrees Celsius for 1 hour, and control the speed at 250-500 rpm to obtain mixture 2;
[0030] ④ Add the...
Embodiment 2
[0033] A white water-based acrylic marker ink consisting of the following components by weight:
[0034] Pangang Oriental Titanium Titanium Dioxide 15.0%, Polyethylene Glycol 1.5%, Polyvinylpyrrolidone 0.5%, Sodium Polyacrylate 2.0%, Octylphenol Polyoxyethylene Ether 2.0%, Dow Acrylic Resin Emulsion 45.0%, Purified Water 34.0%, total weight 100 grams.
[0035] The preparation method of above white water-based acrylic marker pen ink, comprises the following steps:
[0036] ① Weigh each component according to the above weight and proportion, the total weight is 100 grams;
[0037] ② Mix the Pangang Dongfang Titanium Industry titanium dioxide weighed in step ① with pure water, and ultrasonically treat it for 20 minutes to obtain a water-dispersed mixture of titanium dioxide;
[0038] ③ Add the polyethylene glycol and polyvinylpyrrolidone weighed in step ① to the mixture 1 obtained in step ②, stir at 60 degrees Celsius for 1 hour, and control the speed at 250-500 rpm to obtain m...
Embodiment 3
[0042] A white water-based acrylic marker ink consisting of the following components by weight:
[0043] DuPont Chemours Titanium Dioxide 15.0%, Polyethylene Glycol 1.5%, Polyvinyl Alcohol 1.5%, Nonylphenol Polyoxyethylene Ether 2.5%, L-type Polyoxyethylene Polyoxypropylene Block Polymer 2.0%, BASF Zhuangqiao Acrylic Resin emulsion 40.0%, purified water 37.5%, total weight 100 grams.
[0044] The preparation method of above white water-based acrylic marker pen ink, comprises the following steps:
[0045] ① Weigh each component according to the above weight and proportion, the total weight is 100 grams;
[0046]② Mix the DuPont Chemours titanium dioxide weighed in step ① with purified water, and ultrasonically treat it for 10 minutes to obtain a water-dispersed mixture of titanium dioxide;
[0047] ③ Add the polyethylene glycol and polyvinylpyrrolidone weighed in step ① to the mixture 1 obtained in step ②, stir at 80 degrees Celsius for 1 hour, and control the speed at 250-50...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com