Recycled asphalt concrete and preparation method thereof
A technology for recycling asphalt and concrete, applied in the field of resource utilization of construction waste, can solve the problems of cracking temperature, poor viscoelastic performance, and inability to use advanced pavement, and achieve the effect of good air purification and performance optimization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] A high-performance recycled asphalt concrete, comprising the following components by weight: 38 parts of coarse aggregate, 45 parts of old asphalt mixture, 3 parts of iron ore powder, 1.2 parts of SBS modified asphalt and 2 parts of regeneration agent;
[0044] in,
[0045] The particle diameter of described coarse aggregate is 26.5mm, and crushing value is 18%, and water absorption rate is 1.5%;
[0046] In the old asphalt mixture mentioned above,
[0047] Old asphalt mixture with a particle size of 13.2-19mm accounted for 28%;
[0048] Old asphalt mixture with a particle size of 4.75-9.5mm accounts for 15%;
[0049] The old asphalt mixture with a particle size of 0.6-2.36mm accounts for 30%,
[0050] The balance is old asphalt mixture with particle size less than 0.15mm;
[0051] The particle diameter of described iron ore powder is 0.075mm;
[0052] In the regenerant, the particle size of the modified diatomite is 100nm, and the mass ratio of the waste engine oi...
Embodiment 2
[0058] A high-performance recycled asphalt concrete, comprising the following components by weight: 42 parts of coarse aggregate, 55 parts of old asphalt mixture, 5 parts of iron ore powder, 2.5 parts of SBS modified asphalt and 3.5 parts of regeneration agent;
[0059] in,
[0060] The particle diameter of described coarse aggregate is 31.5mm, and crushing value is 25%, and water absorption rate is 2%;
[0061] In the old asphalt mixture mentioned above,
[0062] Old asphalt mixture with a particle size of 13.2-19mm accounted for 36%;
[0063] Old asphalt mixture with a particle size of 4.75-9.5mm accounted for 22%;
[0064] The old asphalt mixture with a particle size of 0.6-2.36mm accounts for 40%,
[0065] The balance is old asphalt mixture with particle size less than 0.15mm;
[0066] The particle diameter of described iron ore powder is 0.15mm;
[0067] In the regenerant, the particle size of the modified diatomite is 500nm, and the mass ratio of the waste engine oil,...
Embodiment 3
[0073] A high-performance recycled asphalt concrete, comprising the following components by weight: 39 parts of coarse aggregate, 46 parts of old asphalt mixture, 3.1 parts of iron ore powder, 1.3 parts of SBS modified asphalt and 2.1 parts of regeneration agent;
[0074] in,
[0075] The particle diameter of described coarse aggregate is 31.5mm, and crushing value is 18%, and water absorption rate is 1.5%;
[0076] In the old asphalt mixture mentioned above,
[0077] Old asphalt mixture with a particle size of 13.2-19mm accounted for 36%;
[0078] Old asphalt mixture with a particle size of 4.75-9.5mm accounted for 22%;
[0079] The old asphalt mixture with a particle size of 0.6-2.36mm accounts for 40%,
[0080] The balance is old asphalt mixture with particle size less than 0.15mm;
[0081] The particle diameter of described iron ore powder is 0.075mm;
[0082] In the regenerant, the particle size of the modified diatomite is 150nm, and the mass ratio of the waste engi...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com