A technology of imitation stone paint and beige stone, applied in the field of imitation beige stone paint and its preparation in Germany, can solve the problem that it cannot be sprayed on the wall at one time, and another color point needs to be sprayed after one point is sprayed. Long time, uncontrollable construction quality and other issues
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0094] First, prepare sintered sand-in-water imitation stone coating:
[0095] 1. Preparation of protective gel solution:
[0096] Put deionized water and protective glue into the mixer at a ratio of 4:1, stir and disperse at 460 rpm for 30 minutes, and store for later use.
[0097] 2. Prepare the dispersed phase:
[0098] (1) Stir the above-mentioned deionized water and cellulose in a disperser for 15 minutes at a speed of 1000 r / min. obtain the first mixture;
[0099] (2) Add dispersant, defoamer, propylene glycol, pH regulator, film-forming aid, emulsion, preservative to the second mixture under the condition of 460r / min;
[0100] (3) Add thickener and protective colloid solution to the second mixture under the condition of 1000r / min to obtain the third mixture;
[0101] (4) The third mixture is added to sintered colored sand under the condition of 460r / min to obtain the dispersed phase;
[0102] The dispersed phase comprises the following components in parts by weight...
Embodiment 2
[0114] First, prepare sintered sand-in-water imitation stone coating:
[0115] 1. Preparation of protective gel solution:
[0116] Put deionized water and protective glue into the mixer at a ratio of 7:1, stir and disperse at 400 rpm for 30 minutes, and store for later use.
[0117] 2. Prepare the dispersed phase:
[0118] (1) Stir the above-mentioned deionized water and cellulose in a disperser for 15 minutes at a speed of 800 r / min. obtain the first mixture;
[0119] (2) Add dispersant, defoamer, propylene glycol, pH regulator, film-forming aid, emulsion, preservative to the second mixture under the condition of 400r / min to the first mixture;
[0120] (3) Add thickener and protective colloid solution to the second mixture under the condition of 800r / min to obtain the third mixture;
[0121] (4) The third mixture is added to sintered colored sand under the condition of 400r / min to obtain the dispersed phase;
[0122] The dispersed phase comprises the following components...
Embodiment 3
[0134] First, prepare sintered sand-in-water imitation stone coating:
[0135] 1. Preparation of protective gel solution:
[0136] Put the deionized water and protective glue into the mixer at a ratio of 3:1, stir and disperse at a speed of 500 rpm for 30 minutes, and store it for later use.
[0137] 2. Prepare the dispersed phase:
[0138] (1) Stir the above-mentioned deionized water and cellulose in a disperser for 15 minutes at a speed of 1500 r / min. obtain the first mixture;
[0139] (2) Add dispersant, defoamer, propylene glycol, pH regulator, film-forming aid, emulsion, preservative to the second mixture under the condition of 500r / min;
[0140] (3) Add thickener and protective colloid solution to the second mixture under the condition of 1500r / min to obtain the third mixture;
[0141] (4) The third mixture is added to the sintered colored sand under the condition of 500r / min to obtain the dispersed phase;
[0142] The dispersed phase comprises the following compone...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com