Embodiment 1
[0025] A kind of preparation method of high bonding strength bamboo plywood that the present invention proposes, comprises the steps:
[0026] S1, bamboo curtain is carried out ultrasonic treatment, the power of ultrasonic treatment is 1200w, the time of ultrasonic treatment is 40min, the frequency of ultrasonic treatment is 15kHz;
[0027] S2, carbonizing the bamboo curtain after ultrasonic treatment, wherein the carbonization treatment is sending the bamboo curtain into a drying and disinfecting carbon dryer, the heating temperature of the drying and disinfecting carbon dryer is 160 ° C, and the heating time is 2 hours, and the bamboo curtain is carbonized. The degree of carbonization is 5%;
[0028] S3, adopt oxygen to carry out plasma treatment to the carbonized bamboo curtain, the time of plasma treatment is 3s, the distance of plasma treatment is 8mm, the power of plasma treatment is 560W, the pressure of plasma treatment is 34Pa, the temperature of plasma treatment is 3...
Embodiment 2
[0035] A kind of preparation method of high bonding strength bamboo plywood that the present invention proposes, comprises the steps:
[0036] S1, bamboo curtain is carried out ultrasonic treatment, the power of ultrasonic treatment is 1500w, the time of ultrasonic treatment is 30min, the frequency of ultrasonic treatment is 30kHz;
[0037] S2, carbonize the bamboo curtain after the ultrasonic treatment, wherein the carbonization treatment is sending the bamboo curtain into a drying and disinfecting carbon dryer, the heating temperature of the drying and disinfecting carbon dryer is 170 ° C, and the heating time is 3 hours, and the bamboo curtain is carbonized. The degree of carbonization is 25%;
[0038]S3, adopt oxygen to carry out plasma treatment to the carbonized bamboo curtain, the time of plasma treatment is 5s, the distance of plasma treatment is 10mm, the power of plasma treatment is 530W, the pressure of plasma treatment is 36Pa, the temperature of plasma treatment i...
Embodiment 3
[0045] A kind of preparation method of high bonding strength bamboo plywood that the present invention proposes, comprises the steps:
[0046] S1, bamboo curtain is carried out ultrasonic treatment, the power of ultrasonic treatment is 1300w, the time of ultrasonic treatment is 45min, the frequency of ultrasonic treatment is 20kHz;
[0047] S2, carbonize the bamboo curtain after the ultrasonic treatment, wherein the carbonization treatment is sending the bamboo curtain into a drying and disinfecting carbon dryer, the heating temperature of the drying and disinfecting carbon dryer is 190 ° C, and the heating time is 4 hours, and the bamboo curtain is carbonized. The degree of carbonization is 30%;
[0048] S3, using oxygen to carry out plasma treatment on the carbonized bamboo curtain, the time of plasma treatment is 3.5s, the distance of plasma treatment is 9mm, the power of plasma treatment is 550W, the pressure of plasma treatment is 34.5Pa, and the temperature of plasma tre...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com