Preparation method of high-nickel ternary material
A high-nickel ternary material, three-stage technology, used in electrical components, electrode manufacturing, electrode heat treatment, etc., can solve the problems of aggravated Li ion diffusion, low initial efficiency and power, and poor material reversibility, and achieve crystallization. High stability, high first efficiency, and the effect of improving crystallinity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0010] The application provides a method for preparing a high-nickel ternary material, the high-nickel ternary material is Li (1+a) Ni x co y m z o 2+b , where, -0.10≤a≤0.50, 0.8≤x<0.9, 0.1≤y≤0.25, 0
[0011] Further, the sintering in the first stage is as follows: the mixture added with the sintering aid is heated up to 650-750°C at a heating rate of 0.5-10°C / min in an air atmosphere, and kept for 3-6h to obtain intermediate I. The first temperature platform is set at a pos...
Embodiment 1
[0029] High nickel ternary material Li 1.01 Ni 0.8 co 0.1 mn 0.1 o 2.005 The preparation method is:
[0030] a. Precursor preparation
[0031] Add metal Ni, Co, Mn sulfate solution, shape control agent ammonia, NaOH solution into the reaction kettle and mix them in parallel, control the pH=12, and react at a constant temperature at 65°C, and continue to react until the particle size D50 is 10um, the precursor Ni was obtained after filtering and washing 0.8 co 0.1 mn 0.1 (OH) 2 ;
[0032] b. mix
[0033] Mix the precursor and lithium hydroxide at a molar ratio of 1:1.10, add boron oxide, an insoluble auxiliary agent accounting for 10% of the mass of the precursor, and mix evenly;
[0034] c. Three-stage sintering
[0035] Carry out the first-stage sintering of the mixed mixture in b: put it in the air atmosphere, raise the temperature to 650°C at a heating rate of 1°C / min, and keep it for 4h to obtain intermediate I;
[0036] Then carry out the second stage of sint...
Embodiment 2
[0039] High nickel ternary material Li 1.01 Ni 0.8 co 0.1 mn 0.1 o 2.005 The preparation method is:
[0040] a. Precursor preparation
[0041] Add the sulfate solution of metal Ni, Co, Mn, shape control agent ammonia, and sodium carbonate solution in the reaction kettle to carry out parallel flow mixing in the reaction kettle, control the pH=12, and react at a constant temperature at 65°C, and continue the reaction until The particle size D50 is 9um, and the precursor Ni is obtained after filtering and washing 0.8 co 0.1 mn 0.1 CO 3 ;
[0042] b. mix
[0043] Mix the precursor and lithium hydroxide at a molar ratio of 1:1.10, add boron oxide, an insoluble auxiliary agent accounting for 10% of the mass of the precursor, and mix evenly;
[0044] c. Three-stage sintering
[0045] Carry out the first-stage sintering of the mixed mixture in b: put it in the air atmosphere, raise the temperature to 650°C at a heating rate of 1°C / min, and keep it for 4h to obtain intermed...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction