A technology of permeable asphalt and admixture, which is applied in the field of permeable asphalt admixture, permeable asphalt and permeable asphalt pavement, can solve the problems of easy blockage of voids, difficult construction and high cost, and achieves fast water permeability, excellent sound absorption and noise reduction effect, and low cost. low effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] The permeable asphalt admixture of this example, the raw materials used for its preparation include the following components by weight: 1.5 parts of emulsifier, 1 part of dispersant, 4 parts of capillary pore forming agent and 0.06 part of catalyst. Wherein, the HLB value of the emulsifier is 8-18, and the emulsifier is alkylphenol polyoxyethylene ether; the dispersant includes polycarboxylic acid dispersant and pyrimidine dispersant, polycarboxylic acid dispersant The polymaleic acid dispersant is used as the dispersant, and the melamine sulfonate formaldehyde condensate is used as the pyrimamine dispersant; the capillary pore forming agent is zinc stearate. The components and specific proportions of the raw materials used for the above-mentioned preparation of the permeable asphalt admixture are shown in Table 1.
[0024] Table 1
[0025]
[0026] The preparation method of the water-permeable asphalt admixture of this embodiment includes: adding the weighed emulsi...
Embodiment 2
[0030] This example is similar to Example 1, wherein the components and specific ratios of the raw materials used to prepare the water-permeable asphalt admixture are shown in Table 2.
[0031] Table 2
[0032]
[0033] The preparation method of the water-permeable asphalt admixture of this embodiment includes: adding the weighed emulsifier, dispersant, capillary pore forming agent, and catalyst into the reaction kettle, polymerizing at 40°C for 5 hours, and then cooling to room temperature, That is, the permeable asphalt admixture is obtained.
[0034] The permeable asphalt admixture is added into the asphalt according to 5% of the weight of the asphalt, stirred and dispersed evenly, and the permeable asphalt is obtained.
[0035] In addition to the above, this embodiment also provides a permeable asphalt pavement, which contains the above-mentioned permeable asphalt admixture.
Embodiment 3
[0037] This example is similar to Example 1, wherein the components and specific ratios of the raw materials used to prepare the water-permeable asphalt admixture are shown in Table 3.
[0038] table 3
[0039]
[0040]
[0041] The preparation method of the water-permeable asphalt admixture of this embodiment includes: adding the weighed emulsifier, dispersant, capillary pore forming agent, and catalyst into the reaction kettle, polymerizing at 50°C for 3 hours, and then cooling to room temperature, That is, the permeable asphalt admixture is obtained.
[0042] The permeable asphalt additive is added into the asphalt according to 6.56% of the weight of the asphalt, stirred and dispersed evenly, and the permeable asphalt is obtained.
[0043] In addition to the above, this embodiment also provides a permeable asphalt pavement, which contains the above-mentioned permeable asphalt admixture.
[0044] Table 4 shows the partial performance comparison results between the pe...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com