Scouring agent for silk fabric and application method of scouring agent
A fabric and silk technology, applied in animal fibers, textiles, papermaking, fiber treatment, etc. It can solve the problems of hard water resistance, high foaming, and poor penetration of scouring agents, and achieve excellent scouring effects. The method is simple and convenient. good refining effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Liquid A: 100 parts of potassium octadecyl diphenyl ether disulfonate, 20 parts of stearyl alcohol polyoxyethylene ether, 8 parts of di-second-octyl maleate sulfonate, 2 parts of chelating dispersant, 4 parts of propynyl alcohol;
[0022] Solution B: 10 parts of papain, 80 parts of pH buffer.
[0023] After diluting liquid A, adjust the pH to 7-9, heat, control the temperature at 50°C, immerse the silk fabric in it, stir slowly, keep it for 90 minutes, take it out and wash it with water once; after diluting liquid B, add it to the fabric, Adjust the pH to 7, maintain the temperature at 60°C, and continue the treatment for 45 minutes, then take it out and wash it with water above 80°C.
Embodiment 2
[0025] Liquid A: 100 parts of potassium octadecyl diphenyl ether disulfonate, 25 parts of stearyl alcohol polyoxyethylene ether, 10 parts of di-second-octyl maleate sulfonate, 4 parts of chelating dispersant, 6 parts of propynyl alcohol;
[0026] Liquid B: 10 parts of papain, 90 parts of pH buffer.
[0027] After diluting liquid A, adjust the pH to 8, heat, control the temperature at 60°C, immerse the silk fabric in it, stir slowly, keep it for 60 minutes, take it out and wash it with water once; after diluting liquid B, add it to the fabric to adjust the pH 6-7, maintain the temperature at 60°C, and continue to treat for 30 minutes, then take it out and wash it with water above 80°C.
Embodiment 3
[0029] Liquid A: 100 parts of potassium octadecyl diphenyl ether disulfonate, 30 parts of stearyl alcohol polyoxyethylene ether, 12 parts of di-second-octyl maleate sulfonate, 5 parts of chelating dispersant, 4 parts of propynyl alcohol;
[0030] Liquid B: 10 parts of papain, 90 parts of pH buffer.
[0031] After diluting liquid A, adjust the pH to 8, heat, control the temperature at 40°C, immerse the silk fabric in it, stir slowly, keep it for 90 minutes, take it out and wash it with water once; after diluting liquid B, add it to the fabric to adjust the pH 7, maintain the temperature at 60°C, continue to treat for 45 minutes, remove and wash with water above 80°C.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com