Multifunctional inorganic interior wall coating and preparation method thereof
An interior wall coating, multi-functional technology, applied in fireproof coatings, antifouling/underwater coatings, alkali metal silicate coatings, etc. Formaldehyde and other organic pollutants, the effect of broad market prospects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0044] The formula of multi-functional interior wall paint is: potassium silicate 9%, lithium silicate 3%, silica sol 13%, diatomaceous earth 9%, shell powder 7%, photosensitizing additive loaded tourmaline powder 11%, anti-radiation- Bactericidal additive loaded bentonite 11%, nano-SiO 2 Dispersion liquid 5%, calcined kaolin 4%, anatase titanium dioxide 6%, alumina powder 4%, water 18%.
[0045] The preparation method is as follows:
[0046] 1. Preparation of Photosensitizing Auxiliary Loaded Tourmaline Powder
[0047] (1) Add tourmaline powder into water according to the weight ratio of solid-liquid ratio of 1:5, stir and mix and carry out ultrasonic dispersion to form tourmaline powder suspension, and add 20% concentration of tourmaline powder to the suspension under stirring Glycine solution to a pH value of 6.0, then filtered, washed, and dried in a constant temperature oven at 60°C to obtain pretreated tourmaline powder;
[0048] (2) According to the volume ratio of e...
Embodiment 2
[0069] The formula of multi-functional interior wall paint is: 15% potassium silicate, 5% lithium silicate, 5% silica sol, 5% diatomaceous earth, 9% shell powder, 15% tourmaline powder loaded with photosensitizing additive, anti-radiation- Bactericidal additive loaded bentonite 5%, nano-SiO 2 Dispersion liquid 10%, calcined kaolin 2%, anatase titanium dioxide 3%, alumina powder 2%, water 24%.
[0070] The preparation method is the same as in Example 1.
Embodiment 3
[0072] The formula of multifunctional interior wall paint is: 5% potassium silicate, 2% lithium silicate, 10% silica sol, 15% diatomaceous earth, 5% shell powder, 5% tourmaline powder loaded with photosensitizing additive, anti-radiation- Bactericidal additive loaded bentonite 15%, nano-SiO 2 Dispersion liquid 2%, calcined kaolin 8%, anatase titanium dioxide 12%, alumina powder 8%, water 13%.
[0073] The preparation method is the same as in Example 1.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com