After-treatment technology of double faced velvet fabric
A double-sided fleece and post-finishing technology, applied in fiber treatment, biochemical fiber treatment, improved hand-feeling fibers, etc., can solve the problem of insufficient softness to the hand, and achieve the effect of soft hand-feel and excellent flame retardancy
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] The post-finishing process of the double-sided fleece fabric includes the following steps:
[0026] 1) 1 to 2 parts by weight of cetyl dimethyl benzyl ammonium chloride, 5.3 parts by weight of stearylamine polyoxyethylene ether, 3.1 parts by weight of dioctadecyl alcohol ester, 6.7 parts by weight of citric acid, 1.3 parts by weight Parts of lauryltrimethylammonium chloride are dropped into 56 parts by weight of deionized water successively, and stirred evenly;
[0027] 2) then drop into 2.3 parts by weight of hydroxypropyl methylcellulose, 1.2 parts by weight of fatty acid methyl ester sulfonate, 4.6 parts by weight of dimethyl fumarate, 2.1 parts by weight of sodium carboxymethylcellulose, 0.9 parts by weight of methylcellulose Base nonyl ketone, continue to stir, until fully mixed, make finishing solution;
[0028] 3) Then pad the fabric in the finishing solution, take it out and dry it at a constant temperature.
Embodiment 2
[0030] The post-finishing process of the double-sided fleece fabric includes the following steps:
[0031] 1) 1 part by weight of cetyl dimethyl benzyl ammonium chloride, 5.3 parts by weight of stearylamine polyoxyethylene ether, 3.1 parts by weight of dioctadecyl alcohol ester, 6.7 parts by weight of citric acid, 1.3 parts by weight of chlorine Add lauryltrimethylammonium into 56 parts by weight of deionized water successively, and stir evenly;
[0032] 2) then drop into 2.3 parts by weight of hydroxypropyl methylcellulose, 1.2 parts by weight of fatty acid methyl ester sulfonate, 4.6 parts by weight of dimethyl fumarate, 2.1 parts by weight of sodium carboxymethylcellulose, 0.9 parts by weight of methylcellulose Base nonyl ketone, continue to stir, until fully mixed, make finishing solution;
[0033] 3) Then pad the fabric in the finishing solution, take it out and dry it at a constant temperature.
Embodiment 3
[0035] The post-finishing process of the double-sided fleece fabric includes the following steps:
[0036] 1) 2 parts by weight of cetyl dimethyl benzyl ammonium chloride, 5.3 parts by weight of stearylamine polyoxyethylene ether, 3.1 parts by weight of dioctadecyl alcohol ester, 6.7 parts by weight of citric acid, 1.3 parts by weight of chlorine Add lauryltrimethylammonium into 56 parts by weight of deionized water successively, and stir evenly;
[0037] 2) then drop into 2.3 parts by weight of hydroxypropyl methylcellulose, 1.2 parts by weight of fatty acid methyl ester sulfonate, 4.6 parts by weight of dimethyl fumarate, 2.1 parts by weight of sodium carboxymethylcellulose, 0.9 parts by weight of methylcellulose Base nonyl ketone, continue to stir, until fully mixed, make finishing solution;
[0038] 3) Then pad the fabric in the finishing solution, take it out and dry it at a constant temperature.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.