A kind of preparation method of glass conductive fiber with cuprous sulfide as conductive layer
A cuprous sulfide and glass fiber technology is applied in the field of composite conductive fiber preparation, which can solve the problems of affecting the adsorption and fastness of metal sulfides, and the inability to obtain conductive fibers, so as to solve the problem of effective adsorption and loss of fiber performance. The effect of less, long-lasting conductive effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] The preparation method of the glass conductive fiber with cuprous sulfide as the conductive layer of the present embodiment, the steps are as follows:
[0021] (1) Immerse 10 grams of cleaned alkali-free glass fiber into 150 grams of hydrochloric acid aqueous solution with a concentration of 2mol / L, soak for 2 hours at 20°C, rinse with water after soaking, and dry the fiber to obtain hydroxylated glass fiber;
[0022] (2) Immerse the hydroxylated glass fiber obtained in step (1) in an aqueous solution of 2% silk fibroin, and soak it at 30°C for 1 hour. Soak for 0.5 hours at ℃, take it out, rinse with water fully, dry the fiber to obtain glass fiber with silk fibroin surface modification;
[0023] (3) Place the silk fibroin surface-modified glass fibers prepared in step (2) in 150 grams of 5% aqueous copper sulfate solution, soak at 60°C for 5 minutes, then add 150 grams of 5% copper sulfate The aqueous solution of sodium thiosulfate is heated up to 85 ℃ and reacted fo...
Embodiment 2
[0025] The preparation method of the glass conductive fiber with cuprous sulfide as the conductive layer of the present embodiment, the steps are as follows:
[0026] (1) Immerse 10 grams of cleaned alkali-free glass fibers in 200 grams of 1mol / L hydrochloric acid aqueous solution, soak for 0.5 hours at 50°C, rinse with water after soaking, and dry the fibers to obtain hydroxylated glass fiber;
[0027] (2) Immerse the hydroxylated glass fibers obtained in step (1) in an aqueous solution of 4% silk fibroin, and soak them at 30°C for 3 hours. Soak for 2 hours at ℃, take it out, rinse it fully with water, dry the fiber to get the glass fiber with silk fibroin surface modification;
[0028] (3) Place the silk fibroin surface-modified glass fibers prepared in step (2) in 150 grams of 2.5% aqueous copper sulfate solution, soak at 60°C for 5 minutes, then add 150 grams of 2.5% copper sulfate The aqueous solution of sodium thiosulfate is heated up to 75°C and reacted for 1.5 hours....
Embodiment 3
[0030] The preparation method of the glass conductive fiber with cuprous sulfide as the conductive layer of the present embodiment, the steps are as follows:
[0031] (1) Immerse 10 grams of cleaned alkali-free glass fibers into 150 grams of hydrochloric acid aqueous solution with a concentration of 1.5 mol / L, and soak for 1.5 hours at 30°C. After soaking, fully rinse with water, and dry the fibers to obtain hydroxylation. fiberglass;
[0032] (2) Immerse the hydroxylated glass fiber obtained in step (1) in a 3% silk fibroin aqueous solution, and soak it at 35°C for 2.5 hours. Soak for 1.5 hours at ℃, take it out and rinse it with water, dry the fiber to obtain glass fiber with silk fibroin surface modification;
[0033] (3) Place the silk fibroin surface-modified glass fibers prepared in step (2) in 150 grams of 8% aqueous copper sulfate solution, soak at 30°C for 20 minutes, then add 300 grams of 4% The aqueous solution of sodium thiosulfate is heated up to 75 ℃ and reacte...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com