A polypropylene-type, multi-layer co-extrusion technology, applied in lamination devices, chemical instruments and methods, lamination, etc., can solve the problem of excessive tensile stress and strain of bonding strength, affecting product quality and production efficiency, and angular edges Solve problems such as delamination, achieve excellent bonding performance, improve product quality and production efficiency, and achieve lasting and stable bonding strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] The raw material formulation of the polypropylene adhesive resin composition for multi-layer co-extruded barrier packaging (the following proportions are weight percent content) is as follows:
[0026] 69% random copolymer polypropylene
[0027] 15% functionalized modified random copolymerized polypropylene
[0028] 13% propylene-based elastomer
[0029] 3% Styrenic Block Copolymer
[0030] 0.08% thermal oxygen stabilizer
[0031] The above-mentioned components are extruded and granulated by plasticizing and blending with a twin-screw extruder. The length-to-diameter ratio of the extruder is L / D=40:1, and the processing temperature is 150-230°C. Polypropylene type adhesive resin for multilayer coextruded barrier packaging.
Embodiment 2
[0033] The raw material formulation of the polypropylene adhesive resin composition for multi-layer co-extruded barrier packaging (the following proportions are weight percent content) is as follows:
[0034] 65% random copolymer polypropylene
[0035] 18% functionalized modified random copolymer polypropylene
[0036] 15% propylene-based elastomer
[0037] 2% Styrenic Block Copolymer
[0038] 0.1% thermal oxygen stabilizer
[0039] The above-mentioned components are extruded and granulated by plasticizing and blending with a twin-screw extruder. The length-to-diameter ratio of the extruder is L / D=40:1, and the processing temperature is 150-230°C. Polypropylene type adhesive resin for multilayer coextruded barrier packaging.
Embodiment 3
[0041] The raw material formulation of the polypropylene adhesive resin composition for multi-layer co-extruded barrier packaging (the following proportions are weight percent content) is as follows:
[0042] 60% random copolymer polypropylene
[0043] 20% functionalized modified random copolymer polypropylene
[0044] 18% propylene-based elastomer
[0045] 2% Styrenic Block Copolymer
[0046] 0.12% thermal oxygen stabilizer
[0047] The above-mentioned components are extruded and granulated by plasticizing and blending with a twin-screw extruder. The length-to-diameter ratio of the extruder is L / D=40:1, and the processing temperature is 150-230°C. Polypropylene type adhesive resin for multilayer coextruded barrier packaging.
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com