A foam material and silicone rubber technology, which is applied in the field of preparation of self-adhesive silicone rubber foam materials, can solve the problems of silicone rubber performance impact, low foaming efficiency, and increasing the types of silicone rubber raw materials, achieving low cost and high foaming efficiency , the effect of fewer types of raw materials
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] (1) Prepare raw materials, the components of raw materials and their weight percentages are as follows:
[0028] Methyl vinyl silicone rubber: 90%
[0029] Hydrophobic vapor phase method white carbon black: 5%
[0030] Methyl silicone oil: 2%
[0031] Blowing agent AC: 1%
[0032] Crosslinking agent DBPMH: 2%
[0033] (2) Put the prepared raw materials into an internal mixer and mix evenly; put the mixture in an open mixer and open the mixer to obtain a mixture sheet with a thickness of 2mm; put the mixture sheet into a closed mold and heat it with a flat vulcanizer. The foamed sheet is obtained; the foamed sheet is subjected to post-heating treatment to obtain a self-adhesive silicone rubber foam board.
[0034] The self-adhesive silicone rubber foam board prepared above is subjected to a mechanical test, and the test result is: the density of the self-adhesive silicone rubber foam board is 350 g / L, and the permanent compression set becomes 2.3%.
[0035] The self-adhesive silicon...
Embodiment 2
[0038] (1) Prepare raw materials, the components of raw materials and their weight percentages are as follows:
[0039] Methyl vinyl silicone rubber: 50%, methyl phenyl silicone rubber: 45%
[0040] Methyl silicone oil: 3%
[0041] Foaming agent: sodium bicarbonate 1%
[0042] Crosslinking agent: dibenzoyl peroxide 1%
[0043] (2) Put the prepared raw materials into an internal mixer and mix evenly; put the mixture in an open mixer and open the mixer to obtain a mixture sheet with a thickness of 2mm; put the mixture sheet into a closed mold and heat it with a flat vulcanizer. The foamed sheet is obtained; the foamed sheet is subjected to post-heating treatment to obtain a self-adhesive silicone rubber foam board.
[0044] The self-adhesive silicone rubber foam board prepared above is subjected to a mechanical test, and the test result is: the density of the self-adhesive silicone rubber foam board is 295 g / L, and the permanent compression set becomes 2.8%.
[0045] The self-adhesive sili...
Embodiment 3
[0048] (1) Prepare raw materials, the components of raw materials and their weight percentages are as follows:
[0049] Methyl vinyl silicone rubber: 45%, fluorosilicone rubber: 45%
[0050] Hydrophobic vapor phase method white carbon black: 2%
[0051] Methyl silicone oil: 4%
[0052] Foaming agent: sodium bicarbonate 2%
[0053] Crosslinking agent: dicumyl peroxide 2%
[0054] (2) Put the prepared raw materials into an internal mixer and mix evenly; place the mixture in an open mixer and open the mixer to obtain a mixture sheet with a thickness of 2 mm; put the mixture sheet into a closed mold and use infrared heating to obtain Foam sheet: After heating the foam sheet, a self-adhesive silicone rubber foam board is obtained.
[0055] The self-adhesive silicone rubber foam board prepared above was subjected to a mechanical test, and the test result was: the density of the self-adhesive silicone rubber foam board was 231 g / L, and the permanent compression set became 3.2%.
[0056] The self...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com