Ultrasoft noiseless feather prevention fabric and fabrication method thereof
A noise-free technology for feather-proof fabrics, applied in textiles, fabrics, fiber types, etc., can solve problems affecting consumers' sleep quality and hard-feeling feather-proof fabrics
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0022] The preparation method of ultra-soft and noiseless anti-feather fabric of the present invention, it comprises the steps:
[0023] Spinning → weaving → windproof soft finishing → drying.
[0024] In the present invention, the warp yarn in the spinning is cotton yarn with a yarn count of 60s-100s, the weft yarn is an ultrafine denier polyester filament with a yarn count of 80D-150D, and its weave structure is 2 upper / 1 lower.
[0025] In the present invention, the windproof and softening finishing is to carry out windproof and softening finishing by padding anti-feather finishing agent. Water-based softener KF-896 is compounded; The scrap rate of the anti-feather finishing agent is 70%.
[0026] In the present invention, the drying temperature is 100-120°C, and the drying time is 40-60s.
Embodiment 1
[0028] Process steps:
[0029] Spinning → weaving → windproof soft finishing → drying.
[0030] In the spinning, the warp yarn is cotton yarn with a yarn count of 60s, the weft yarn is an ultra-fine denier polyester filament with a yarn count of 80D, and its weave structure is 2 upper / 1 lower.
[0031] The windproof and softening finishing is to carry out the windproof and softening finishing by padding and anti-feather finishing agent, and the said feather-proof finishing agent is TK-803 of special aliphatic polymer compound emulsion King-tech containing organic silicon and hydrophilic softener KF -896 composite; The scrap rate of the anti-feather finishing agent is 70%.
[0032] The drying temperature is 100° C. and the drying time is 40 s.
[0033] The dimensional change rate of the prepared ultra-soft and noise-free feather-proof fabric is ≤5.0% in warp direction and ≤5.0% in weft direction; the amount of drill down is ≤30 strands / cm 2 .
Embodiment 2
[0035] Process steps:
[0036] Spinning → weaving → windproof soft finishing → drying.
[0037] In the spinning, the warp yarn is cotton yarn with a yarn count of 100s, the weft yarn is an ultrafine denier polyester filament with a yarn count of 150D, and its weave structure is 2 upper / 1 lower.
[0038] The windproof and softening finishing is to carry out the windproof and softening finishing by padding and anti-feather finishing agent, and the said feather-proof finishing agent is TK-803 of special aliphatic polymer compound emulsion King-tech containing organic silicon and hydrophilic softener KF -896 composite; The scrap rate of the anti-feather finishing agent is 70%.
[0039] The drying temperature is 120° C. and the drying time is 60 s.
[0040] The dimensional change rate of the prepared ultra-soft and noise-free feather-proof fabric is ≤5.0% in warp direction and ≤5.0% in weft direction; the amount of drill down is ≤30 strands / cm 2 .
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com