Embodiment 1
[0026] A method for manufacturing sublimation transfer printing paper base paper, comprising the steps of:
[0027] Step 1: 5 parts by weight of coniferous wood (Massonia pine) pulp board and 5 parts by weight of hardwood (birch) pulp board are pulped separately with a hydraulic pulper, and then beaten to 15°SR by serial double disc mills and 18°SR;
[0028] Step 2: Pump the above two kinds of pulp after beating to the mixing tank for full mixing to obtain a mixed pulp, and then mix it with poplar CTMP chemical mechanical pulp that has been beaten to 22°SR in advance, and make a mixed pulp according to the weight ratio: CTMP chemical mechanical pulp The ratio of slurry=8:2 is mixed to obtain the total mixed slurry;
[0029] Step 3, send the above-mentioned total mixed slurry into the stainless steel mixing tank, add wet strength agent polyamide epoxy resin (PAE), alum and sizing agent cationic rosin glue, the amount of wet strength agent added is 5% of the dry slurry weight ...
Embodiment 2
[0032] A method for manufacturing sublimation transfer printing paper base paper, comprising the steps of:
[0033] Step 1: Pulping 5 parts by weight of softwood (lark) pulp board and 5 parts by weight of hardwood (poplar) pulp board with a hydraulic pulper, and then beating them to 25° with a series double disc mill SR and 28°SR;
[0034] Step 2: Pump the above two kinds of pulp after beating to the mixing tank for full mixing to obtain a mixed pulp, and then mix it with poplar CTMP chemical mechanical pulp that has been beaten to 32°SR in advance, and make a mixed pulp according to the weight ratio: CTMP chemical mechanical pulp The ratio of slurry=6:4 is mixed to obtain the total mixed slurry;
[0035] Step 3, send the above-mentioned total mixed slurry into the stainless steel mixing tank, add wet strength agent polyamide epoxy resin (PAE), alum and sizing agent cationic rosin glue, the amount of wet strength agent added is 5% of the dry slurry weight , the alum addition...
Embodiment 3
[0038] A method for manufacturing sublimation transfer printing paper base paper, comprising the steps of:
[0039] Step 1: 5 parts by weight of coniferous wood (red pine) pulp board and 5 parts by weight of hardwood (basswood) pulp board are pulped with a hydraulic pulper, and then beaten to 20° with a series double disc mill SR and 22°SR;
[0040] Step 2: Pump the above two kinds of pulp after beating to the mixing tank for full mixing to obtain a mixed pulp, and then mix it with poplar CTMP chemical mechanical pulp that has been beaten to 25°SR in advance, and make a mixed pulp according to the weight ratio: CTMP chemical mechanical pulp The ratio of pulp=8:4 is mixed to obtain the total mixed pulp;
[0041] Step 3, send the above-mentioned total mixed slurry into the stainless steel mixing tank, add wet strength agent polyamide epoxy resin (PAE), alum and sizing agent cationic rosin glue, the amount of wet strength agent added is 3% of the dry slurry weight , the alum ad...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com