One-step production of barium hydroxide and sodium sulfide by using barium sulfide and sodium hydroxide
A barium hydroxide and sodium hydroxide technology, applied in the direction of alkali metal sulfide/polysulfide, calcium/strontium/barium oxide/hydroxide, etc. Product purity impact and other issues, to achieve the effect of saving raw material hydrochloric acid, no pollution to the environment, and shortening the process route
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] The industrial barium sulfide black ash that 2kg barium sulfide content is 65% is packed in the container that is used for leaching, adds 3.5L hot water to this container, and the temperature of described hot water is above 95 ℃. During the leaching process, the container can be heated to ensure the water temperature.
[0027] In the above steps, on the one hand, the leaching of the raw material is repeated until the content of barium sulfide in the raw material residue is lower than 1%. On the other hand, for the leaching solution whose concentration needs to be lower than 20°Be, it is added into the container cyclically as the leaching solution to leach the raw material.
[0028] After the leaching is completed, remove the slag from the leaching solution, add it to the tank, let it stand, keep warm at 95°C, and concentrate to above 30°Be.
[0029] Add the leaching solution after standing for heat preservation into the reaction tank, measure the amount of barium ions ...
Embodiment 2
[0033] The industrial barium sulfide black ash that 2kg barium sulfide content is 55% is packed in the container that is used for leaching, adds 3.5L hot water to this container, and the temperature of described hot water is above 70 ℃. During the leaching process, the container can be heated to ensure the water temperature.
[0034] In the above steps, on the one hand, the leaching of the raw material is repeated until the content of barium sulfide in the raw material residue is lower than 1%. On the other hand, for the leaching solution whose concentration needs to be lower than 20°Be, it is added into the container cyclically as the leaching solution to leach the raw material.
[0035] After the leaching is completed, remove the slag from the leaching solution, add it to the tank, let it stand, keep warm at 80°C, and concentrate to above 30°Be.
[0036] Add the leaching solution after standing for heat preservation into the reaction tank, measure the amount of barium ion i...
Embodiment 3
[0040] The industrial barium sulfide black ash that 2kg barium sulfide content is 60% is packed in the container that is used for leaching, adds 3.5L hot water to this container, and the temperature of described hot water is above 90 ℃. During the leaching process, the container can be heated to ensure the water temperature.
[0041] In the above steps, on the one hand, the leaching of the raw material is repeated until the content of barium sulfide in the raw material residue is lower than 1%. On the other hand, for the leaching solution whose concentration needs to be lower than 20°Be, it is added into the container cyclically as the leaching solution to leach the raw material.
[0042] After the leaching is completed, remove the slag from the leaching solution, add it to the tank, let it stand, keep warm at 90°C, and concentrate to above 30°Be.
[0043] Add the leaching solution after standing for heat preservation into the reaction tank, measure the amount of barium ions ...
PUM

Abstract
Description
Claims
Application Information

- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com