Method for preparing zeolite socony mobile-5 (ZSM-5) molecular sieve membrane reactor loaded with Cu/stainless steel screen mesh catalyst
A ZSM-5, membrane reactor technology, applied in chemical instruments and methods, physical/chemical process catalysts, chemical/physical/physical chemical processes, etc., to achieve easy processing, high mechanical strength, and good ductility.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] Process the stainless steel wire mesh into the required specifications, make it into a honeycomb shape, and wash it in a detergent solution with a concentration of 0.075wt% for 15 minutes at 50°C to remove the oil on the surface of the stainless steel wire mesh;
[0034] Soak the above-mentioned stainless steel wire mesh in 15wt% dilute hydrochloric acid for 15 minutes to remove scale;
[0035] Vibrate the activated stainless steel wire mesh under ultrasonic conditions for 15 minutes;
[0036] The pretreated stainless steel wire mesh was completely submerged in 20 wt% H 2 SO 4 In the electrolyte solution, the current density is controlled at 0.80A / dm 2 , the voltage is 3.0V, the time is 20min, and the stainless steel wire mesh with porous structure is obtained;
[0037] Metal copper is used as the anode, the anodized stainless steel wire mesh is used as the cathode, and the electrolyte is 10wt% CuSO 4 solution, the electrodeposition voltage is 1V, and the time is 1m...
Embodiment 2
[0042] Process the stainless steel wire mesh into the required specifications, make it into a honeycomb shape, and wash it in a detergent solution with a concentration of 0.10wt% for 20 minutes at 55°C to remove the oil on the surface of the stainless steel wire mesh;
[0043] Soak the above-mentioned treated stainless steel wire mesh in 15wt% dilute hydrochloric acid for 20 minutes to remove scale;
[0044] Vibrate the activated stainless steel wire mesh under ultrasonic conditions for 20 minutes;
[0045] The pretreated stainless steel wire mesh was completely submerged in 20 wt% H 2 SO 4 In the electrolyte solution, the current density is controlled at 1.00A / dm 2 , the voltage is 3.5V, the time is 25min, and the stainless steel wire mesh with porous structure is obtained;
[0046] Metal copper is used as the anode, the anodized stainless steel wire mesh is used as the cathode, and the electrolyte is 10wt% CuSO 4 solution, the voltage of electrodeposition is 2V, and the ...
Embodiment 3
[0051] Process the stainless steel wire mesh into the required specifications, make it into a honeycomb shape, and wash it in a detergent solution with a concentration of 0.15wt% for 25 minutes at 60°C to remove the oil on the surface of the stainless steel wire mesh;
[0052] Soak the above-mentioned stainless steel wire mesh in 15wt% dilute hydrochloric acid for 25 minutes to remove scale;
[0053] Shake the activated stainless steel wire mesh under ultrasonic conditions for 25 minutes;
[0054] The pretreated stainless steel wire mesh was completely submerged in 20 wt% H 2 SO 4 In the electrolyte solution, the current density is controlled at 1.20A / dm 2 , the voltage is 4.0V, the time is 30min, and the stainless steel wire mesh with porous structure is obtained;
[0055] Metal copper is used as the anode, the anodized stainless steel wire mesh is used as the cathode, and the electrolyte is 10wt% CuSO 4 solution, the electrodeposition voltage is 3V, and the time is 15min...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com