Rubberized asphalt non-cured water-proof coating and preparation process thereof
A preparation process, non-curing technology, used in asphalt coatings, unspecified rubber coatings, coatings, etc., can solve the problems of thermal expansion and contraction joints of waterproof coatings, building deformation joints, and non-curing coatings, so as to improve the weathering resistance. The effect of ability, self-healing enhancement, and simple construction process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] Embodiment 1 selects each raw material by following raw material and weight percentage proportioning
[0019] Rubber 25%
[0020] Carbon black 19%
[0022] Bitumen 47%
[0023] Accelerator 2%
[0024] Binder 5%
[0025] The preparation process requirements are as follows:
[0026] Heat rubber, carbon black, zinc oxide, asphalt, and accelerator in a reaction kettle at 100-190°C, stir for one hour, then add binder, stir for ten minutes, and then put them into a sealed plastic bucket to obtain rubber Vulcanized asphalt non-curing coating.
Embodiment 2
[0027] Embodiment 2 selects each raw material by following raw material and percentage by weight proportioning
[0028] Rubber 22%
[0029] Carbon black 20%
[0031] Bitumen 48%
[0032] Accelerator 2%
[0033] Binder 6%
[0034] The preparation process requirements are as follows:
[0035] Heat rubber, carbon black, zinc oxide, asphalt, and accelerator in a reaction kettle at 100-190°C, stir for one hour, then add binder, stir for ten minutes, and then put them into a sealed plastic bucket to obtain rubber Vulcanized asphalt non-curing coating.
Embodiment 3
[0036] Embodiment 3 selects each raw material by following raw material and weight percentage proportioning
[0037] Rubber 27%
[0038] Carbon black 20%
[0040] Bitumen 40%
[0041] Accelerator 1%
[0042] Binder 7%
[0043] The preparation process requirements are as follows:
[0044] Heat rubber, carbon black, zinc oxide, asphalt, and accelerator in a reaction kettle at 100-190°C, stir for one hour, then add binder, stir for ten minutes, and then put them into a sealed plastic bucket to obtain rubber Vulcanized asphalt non-curing coating.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com