A powder coating and storage-resistant technology, applied in powder coatings, coatings and other directions, can solve the problems of large-scale production obstacles of enterprises, impact on economic benefits of enterprises, and high production costs, so as to increase economic benefits of enterprises and reduce production costs. , the effect of saving energy

Inactive Publication Date: 2010-05-19
FUJIAN WANAN IND
View PDF0 Cites 10 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] In the prior art, powder coatings have long been poorly cured at primary low temperature, and the usual storage period is more than one month. During storage and long-distance transportation, powder coatings are prone to agglomeration and cannot be used, so that the production costs of enterprises remain high. , which brings great obstacles to the large-scale production of enterprises and has a serious impact on the economic benefits of enterprises

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0030] The storage-resistant low-temperature curing powder coating of the present invention is composed of the following raw materials in weight percentage:

[0031] Epoxy resin with a molecular weight of 1600-1900 33%

[0032] Modified polyester resin 26%

[0033] Acrylic acid 0.6%

[0034] Phosphite 0.1%

[0035] Pigments and fillers 37%

[0036] W-187 low temperature curing agent 3%

[0037] R242 quaternary ammonium salt 0.3%

[0038] Its preparation steps are as follows:

[0039] (1) The raw material epoxy resin, modified polyester resin, acrylic acid, phosphite, pigments and fillers, curing agent, curing accelerator are all mixed;

[0040] (2) heating and melting extrusion;

[0041] (3) Tablet cooling;

[0042] (4) Broken and crushed ACM;

[0043] (5) sieve to obtain the product of the present invention when the fineness reaches 180 mesh: storage-resistant low-temperature curing powder coating.

[0044] (6) Finished product packaging.

[0045] The outstanding e...

Embodiment 2

[0047] The storage-resistant low-temperature curing powder coating of the present invention is composed of the following raw materials in weight percentage:

[0048] Epoxy resin with a molecular weight of 1500-1650 32%

[0049] Modified polyester resin 28%

[0050] Acrylic acid 0.6%

[0051] Phosphite 0.1%

[0052] Pigments and fillers 38%

[0053] W-187 low temperature curing agent 1.1%

[0054] R242 quaternary ammonium salt 0.2%

[0055] Its preparation steps are as follows:

[0056] (1) The raw material epoxy resin, modified polyester resin, acrylic acid, phosphite, pigments and fillers, curing agent, curing accelerator are all mixed;

[0057] (2) heating and melting extrusion;

[0058] (3) Tablet cooling;

[0059] (4) Broken and crushed ACM;

[0060] (5) sieve to obtain the product of the present invention when the fineness reaches 180 mesh: storage-resistant low-temperature curing powder coating.

[0061] (6) Finished product packaging.

[0062] The outstanding...

Embodiment 3

[0064] The storage-resistant low-temperature curing powder coating of the present invention is composed of the following raw materials in weight percentage:

[0065] Epoxy resin with a molecular weight of 1400-1600 39%

[0066] Modified polyester resin 29%

[0067] Acrylic acid 0.8%

[0068] Phosphite 0.1%

[0069] Pigment and filler 30%

[0070] W-187 low temperature curing agent 1.0%

[0071] R242 quaternary ammonium salt 0.1%

[0072] Its preparation steps are as follows:

[0073] (1) The raw material epoxy resin, modified polyester resin, acrylic acid, phosphite, pigments and fillers, curing agent, curing accelerator are all mixed;

[0074] (2) heating and melting extrusion;

[0075] (3) Tablet cooling;

[0076] (4) Broken and crushed ACM;

[0077] (5) sieve to obtain the product of the present invention when the fineness reaches 180 mesh: storage-resistant low-temperature curing powder coating.

[0078] (6) Finished product packaging.

[0079] The outstanding e...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a storable low temperature cured powder coating and a preparation method thereof. The powder coating mainly comprises 30 to 40 percent of epoxy resin, 19 to 29 percent of modified polyester resin, 0.5 to 1.2 percent of acrylic acid, 0.08 to 0.15 percent of phosphite ester, 20 to 38 percent of pigment and filler, 0.2 to 3 percent of W-187 low temperature curing agent, and 0.15 to 0.6 percent of curing accelerator. The method for preparing the powder coating comprises the following steps: mixing, heating, melting, extruding, tabletting, cooling, crushing, ACM-crushing and sieving all the raw materials to achieve the fineness of 180 meshes, and packing a finished product. The storage time of the powder coating is greatly prolonged, and the curing temperature is reduced; the powder coating has excellent performance, and is widely applied to surface coating and painting of hardware, electric appliances, home appliances, automobiles, furniture, mechanical equipment and the like; the energy is reduced and the using cost is reduced, so the production cost of enterprises is reduced; and the method ensures the large-scale production of the enterprises, and increases the economic benefits of the enterprises.

Description

Technical field [0001] The invention belongs to the technical field of surface coating and coating, in particular, the invention relates to a low-temperature curing powder coating and a preparation method thereof. Background technique [0002] In the prior art, powder coatings have long been poorly cured at primary low temperature, and the usual storage period is more than one month. During storage and long-distance transportation, powder coatings are prone to agglomeration and cannot be used, so that the production costs of enterprises remain high. , It brings great obstacles to the large-scale production of enterprises, and has a serious impact on the economic benefits of enterprises. Contents of the invention [0003] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a storage-resistant low-temperature curing powder coating with long storage period, low curing temperature and excellent performance ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09D4/06C09D5/03
Inventor 苏捷
Owner FUJIAN WANAN IND
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products