Method for continuous low temperature sintering of high thermal coefficient AIN ceramics and product thereof
A high thermal conductivity, low-temperature sintering technology, which is applied in the field of microelectronic packaging materials and ceramic materials, can solve the problems that are not suitable for large-scale industrial production, hinder the thermal conductivity of aluminum nitride ceramics, and the liquid phase is not easy to be completely eliminated. Low cost, reduced grain boundary phase, and reduced energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Take LiCO 3 、Er 2 o 3 As a sintering aid, polyvinyl butyral (PVB) is used as a coupling agent, dibutyl phthalate (DBP) is used as a plasticizer, OP-83 is used as a dispersant, and toluene is used as a solvent. Take 1Kg powder as an example , whose proportions are as follows:
[0031] AlN 900g
[0032] Nano-AlN 60g
[0033] LiCO 3 15g
[0034] Er 2 o 3 25g
[0035] PVB 100g
[0036] DBP 20g
[0037] OP-83 5g
[0038] Toluene 400g
[0039] AlN powder, nano-AlN (Nano-AlN) powder, sintering aids and rare earth metal oxides, as well as linking agent polyhexene butyral and plasticizer dibutyl phthalate prepared according to the percentage by weight Add the dispersant OP-83 to the solvent toluene together; weigh each material and put it into a ball mill tank for ball milling for 20 hours, and then become AlN slurry after defoaming and aging, and the solid content of the slurry is controlled at about 75%; then The AlN slurry is tape-cast in...
Embodiment 2
[0046] CaCO 3, Y 2 o 3 As a sintering aid, polyvinyl butyral (PVB) is used as a coupling agent, dibutyl phthalate (DBP) is used as a plasticizer, OP-83 is used as a dispersant, toluene is used as a solvent, and 1Kg of powder is used as For example, the proportions are as follows:
[0047] AlN 870g
[0048] Nano-AlN 100g
[0049] CaCO 3 10g
[0050] Y 2 o 3 20g
[0051] PVB 100g
[0052] DBP 20g
[0053] OP-83 5g
[0054] Toluene 400g
[0055] AlN powder, nano-AlN powder, sintering aids and rare earth metal oxides prepared in percentage by weight, as well as coupling agent polyhexene butyral, plasticizer dibutyl phthalate and dispersant OP- 83 was added to the solvent toluene; weigh each material and put it into a ball mill tank for ball milling for 30 hours, and then become AlN slurry after defoaming and aging, and the solid content of the slurry was controlled at about 75%; then the AlN slurry was cast It is formed into a film tape of 1mm; the tap...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology