Process for repairing continuous casting crystal roller
A repair method, continuous casting and crystallization technology, applied in metal material coating process, molten spraying, coating, etc., can solve the problem of affecting the thermal conductivity and mechanical properties of the crystallization roller, the change of the thin strip continuous casting process, the repair area Problems such as high oxygen content, achieve the effect of full roll surface repair, low repair cost, and partial repair
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] In one embodiment of the present invention, the surface of the CrZrCu alloy crystal roller is repaired. The specific operation method is as follows:
[0032] 1. Repair of pits on the surface of CrZrCu alloy crystallization rollers: use mechanical methods to clean up the residues on the surface of pits until new matrix materials appear and there are no cracks. According to the size of the pit, determine the weight of the metal that needs to be melted. On the basis of considering the yield of the metal atomized deposition, it is also necessary to consider that the margin is between 8 and 15%;
[0033] 2. Put the crystal roller that needs to be repaired into the deposition chamber, carry out the repair by spray deposition method, and operate as follows:
[0034] a. Select the CrZrCu alloy with the same composition as the base material for spray atomization deposition, and control its superheat to 120°C after melting;
[0035] b. Vacuumize the deposition chamber to make t...
Embodiment 2
[0044] In the second embodiment of the present invention, the CrZrCu alloy crystal roll surface wear layer is repaired, the crystal roll diameter is 800mm, and the roll body length is 1100mm. The specific operation method is as follows:
[0045] 1. Using a mechanical method, turn the residue on the surface of the crystallization roller to make it appear new matrix material without defects on the surface. At the same time, determine the weight of the metal to be melted according to the wear amount of the crystallization roller, the diameter of the roller, and the length of the roller body. On the basis of the yield of metal atomization deposition, it is also necessary to consider that the margin is between 10 and 25%;
[0046] 2. Put the crystal roller that needs to be repaired into the deposition chamber, carry out the repair by spray deposition method, and operate as follows:
[0047] a. Select the melted CrZrCu alloy with the same composition as the base material for spray a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com