Nylon powder used for high-speed laser sintered products
A nylon powder and laser sintering technology, which is applied in the field of nylon powder materials, can solve the problems of high manufacturing cost, complicated process, and easy damage, and achieve the effects of reducing development costs, good toughness, and strong competitiveness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] (1) Take 1 kg of nylon 12 pellets and cool them to -60°C--150°C in a freezer, then pulverize and sieve to obtain nylon powder;
[0021] (2) With the above-mentioned nylon powder in a high-speed mixer, utilize spray equipment to add surfactant: 1 gram of sodium dodecylbenzenesulfonate, light absorber: light stabilizer 2002, 0.1 gram, after high-speed stirring evenly drying in a vacuum oven to obtain the base material;
[0022] (3) Adding compatibilizer in above-mentioned base material: polypropylene-grafted maleic acid intoxicated 5 grams, viscosity reducing agent: white carbon black 0.5 gram, nucleating agent: nano silicon dioxide 1 gram, filler: polypropylene 5 grams of powder, mixed uniformly in a high-speed mixer, and sieved to obtain nylon powder material.
Embodiment 2
[0023] Embodiment 2: (following detailed process step is with embodiment 1)
[0024] (1) Get 1 kilogram of nylon 6 pellets, freeze, pulverize, and sieve;
[0025] (2) Add surfactant: 10 grams of sodium methylene diisopropylbenzene sulfonate, light absorber: UV327, 5 grams, stir and dry;
[0026] (3) Add compatibilizer: 200 grams of polyethylene-grafted maleic acid, viscosity reducer: 30 grams of calcium carbonate, nucleating agent: 20 grams of nano-alumina, filler; 100 grams of polyethylene powder, mix, sieve point.
Embodiment 3
[0028] (1) Get 1 kilogram of nylon 1010 pellets, freeze, pulverize, and sieve;
[0029] (2) Add surfactant: 2 grams of sodium dialkylsulfonate, light absorber: light stabilizer 2002, 2 grams, stir and dry;
[0030] (3) Add compatibilizer: polypropylene-grafted maleic acid 60 grams, viscosity reducer: white carbon black 20 grams, nucleating agent: nano silicon dioxide 3 grams, filler: polypropylene powder 20 grams, mix , Screening.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com